Aerogel preparation method based on hydrothermal surface modification
Through the hydrothermal surface modification method, the problem of high cost of preparing silica aerogels in water glass is solved. The surface methylation modification is carried out by using acid liquid and high boiling point modifiers, and combined with appropriate drying conditions, low cost is achieved , high-quality and stable aerogel preparation reduces production safety risks and overall costs.
Patent Information
- Application Number
- CN202310580434.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
The cost of preparing silica aerogels in existing water glass is high, mainly because the use of high-energy-consuming organic solvents and a variety of chemical raw materials is required during solvent replacement and surface chemical modification, resulting in unstable product quality and high production costs.
Using hydrothermal surface modification method, by soaking inorganic oxide hydrogel in acid solution and performing surface methylation modification, combining high boiling point modifiers and appropriate drying conditions, avoiding the use of alcohol solvents and reducing production Cost and improve product quality stability.
Aerogel preparation with low cost and stable quality is achieved, reducing production safety risks, and reducing overall production costs by improving surface modification efficiency and material reuse.
Smart Images

Figure HSA0000296982340000011
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing aerogel based on hydrothermal surface modification, and in particular to a method for obtaining aerogel by using inorganic oxide hydrogel as a basic material, performing modification and solvent replacement simultaneously under hydrothermal conditions, and finally drying. Background Art
[0002] At present, the steps of making silica aerogel using water glass mainly include two steps: one is to form silica hydrogel, and the other is to dry the silica hydrogel under the condition that the volume of the final product hardly shrinks.
[0003] There are two main methods for preparing silica hydrogel using water glass. One is to neutralize the water glass with acid to form a gel, and then remove the soluble inorganic salts by washing, as proposed by the inventor Kistler. The second is to pass the diluted water glass through an ion exchange resin to obtain a silica sol with sodium ions removed, and then adjust the pH to obtain a silica hydrogel. Both methods have industrial products, such as dry silica gel and silica sol, so the cost is acceptable to the market.
[0004] However, the cost of silica aerogel using water glass is still not low, mainly due to the subsequent solvent replacement and surface chemical modification.
[0005] The key to solvent replacement is to replace the water in the silica hydrogel with an organic solvent with low surface tension. Since amorphous silica will dissolve and crystallize in high-temperature water, it is not feasible to directly dry the silica aerogel with supercritical water. For the atmospheric pressure drying method, a low surface tension liquid is required to reduce the gel shrinkage caused by the drying process. The surface tension of water is too large, and drying will cause excessive shrinkage of the gel, resulting in the destruction of the gel skeleton structure. Therefore, using a low surface tension organic solvent to replace the water in the silica hydrogel is almost a necessary process for preparing high-quality aerogels.
[0006] Kistler's method requires the use of organic solvents that are miscible with water, such as ethanol, to replace most of the water in the silica hydrogel before supercritical drying can be performed. Because the replacement process takes too long, in the 1970s, Teichner's research group used tetramethoxysilane to produce silica methanol gel. This method of synthesizing silica gel using organosilanes has become the mainstream method for aerogel production. In addition to the long replacement time, Kistler's replacement method requires the water-miscible organic solvent to be dehydrated and recycled for reuse in industrial production. The energy consumption and material loss of ethanol distillation and dehydration are too high, and the overall cost is not even much lower than the cost of directly using organosilanes as raw materials.
[0007] Surface chemical modification is to remove part of the silanol groups on the surface of silica by reacting with organic groups and covering the unreacted silanol groups, so as to avoid contact and condensation of silanol groups caused by gel shrinkage during the drying process, which eventually causes irreversible volume shrinkage of the gel. In addition, methyl modification can also increase the contact angle between the liquid and the gel, reducing the capillary tension. Although the silica gel after solvent replacement and surface modification will still shrink during the drying process, it will rebound after drying, and obtain an aerogel comparable to that obtained by supercritical drying. In addition, some scholars have also adopted an all-in-one atmospheric pressure drying method including surface modification and replacement, which can complete the replacement of water by solvent while modifying the surface. In addition, the process of making aerogel by surface modification is not limited to silica, but can also be applied to other types of inorganic oxides.
[0008] A big problem with the current technical route of drying aerogels at normal pressure is that the replacement and surface modification processes often mix multiple chemical raw materials. In particular, alcohol is needed as a solubilizer to increase the solubility of the modifier in water. After each use, the replacement fluid and modifier components will change to a certain extent, which will lead to unstable product quality next time. If separation and purification are performed every time, the energy consumption cost is also very high. Therefore, even if aerogels are dried at normal pressure, the cost is still not low. In addition, the normal pressure method often uses trimethylsiloxane for modification, and there are relatively few studies on surface modification using dimethylsiloxane.
[0009] The present invention hopes to provide a new method for preparing aerogel with relatively low cost and stable quality. Summary of the invention
[0010] The purpose of the present invention is to provide a method for preparing aerogel based on hydrothermal surface modification, which has low raw material cost, simple process, stable product quality, can avoid the use of alcohol, and reduce production safety risks.
[0011] In order to achieve the above object, the technical solution adopted by the present invention is:
[0012] In the first step, the low-salt inorganic oxide hydrogel is first soaked in an acid solution.
[0013] According to the present invention, the inorganic oxide is amorphous silicon dioxide, titanium dioxide, zirconium dioxide, hafnium dioxide, and a combination of the above-mentioned substances. The above-mentioned inorganic oxide hydrogel can be obtained by hydrolysis of alcohol salts of corresponding elements, or by acid-base neutralization of inorganic salt solutions of corresponding elements to obtain the corresponding hydrogel. Whether the hydrogel is formed by hydrolysis of alcohol salts or neutralization of inorganic salts, a low-salt hydrogel can be obtained by washing with deionized water. Inorganic salts that account for less than 0.2% of the total hydrogel mass can be regarded as a low-salt hydrogel.
[0014] According to the present invention, the hydrogel may contain silicon dioxide, titanium dioxide, silicon carbide, zirconium dioxide, aluminum oxide, graphite, carbon black powder; and aluminum silicate fiber, glass fiber, pre-oxidized fiber, high silica glass fiber, polycrystalline mullite fiber, zirconium oxide fiber, aluminum oxide fiber, polyimide fiber, polyamide fiber, polyester fiber, cellulose fiber, melamine foam. The composite hydrogel can be obtained by uniformly dispersing the above-mentioned powder and fiber materials in the sol stage, or injecting the above-mentioned fiber and foam materials as a substrate into the sol, and waiting for gelation. The size of the powder is preferably 0.5-8μm, and the fiber diameter is preferably 2-15μm.
[0015] According to the present invention, the acid solution is an aqueous solution of hydrochloric acid, hydrobromic acid, hydroiodic acid, and sulfuric acid, and the hydrogen ion concentration is greater than 1 mol / L. Too low acidity cannot achieve an ideal catalytic effect, that is, the surface modification degree and speed cannot meet the requirements of the atmospheric pressure method for synthesizing aerogels.
[0016] In the second step, the acid hydrogel soaked in the acid solution is soaked in a modifier.
[0017] According to the present invention, the modifier includes octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, hexamethyldisiloxane, octamethyltrisiloxane, dimethylcyclosiloxane mixed ring body, dimethyldichlorosilane hydrolyzate, alkane or aromatic hydrocarbon with carbon number of 6-16, and a combination of the above multiple substances. Siloxane with a flash point greater than 28°C is preferably used as the modifier. Alkane or aromatic hydrocarbon with a flash point greater than 28°C is preferably used as the solvent.
[0018] In the third step, the modifier containing the acidic hydrogel is heated to perform surface methylation modification.
[0019] According to the present invention, the surface methylation modification temperature is 60-150°C, preferably from low to high, gradually increasing the temperature. Although the higher the temperature, the faster the modification speed, too high a temperature at the beginning will cause the inorganic oxide gel solubility to be too high, resulting in a significant decrease in specific surface area. Too low a temperature will result in too low a surface modification rate and a low degree of surface modification. Therefore, the surface methylation modification temperature is preferably from low to high, gradually increasing the temperature for heating and modification.
[0020] The fourth step is to remove the acid from the heating system in a timely manner during the surface methylation modification process.
[0021] As the degree of surface methylation increases, the gel will gradually become lipophilic and hydrophobic. Since the acid is incompatible with the modifier, the gel will tend to adsorb the modifier and continuously discharge the acid, gradually completing the solvent replacement. Because the density of the acid is greater than the density of the modifier, the acid will gather at the bottom of the container to form a layer. The gel, due to its lipophilicity, will mainly gather in the upper non-polar liquid, such as Figure 1However, if there is too much acid and part of the gel is submerged, it will directly affect the subsequent surface modification and solvent replacement of this part of the submerged gel. Therefore, it is necessary to remove the acid from the heating system in time.
[0022] In the fifth step, when the lower layer of acid is no longer noticeable, the residual water in the gel is removed by distillation.
[0023] Since the solvent exchange process cannot drive out or react all the water in the gel, especially when the gel size is large, it is necessary to remove the residual water in the gel by distillation. This is to prepare for more thorough surface modification.
[0024] Step 6: Continue to keep the modifier containing the gel warm.
[0025] According to the present invention, the heat preservation temperature is 100-350° C. Properly increasing the temperature can further improve the degree of modification of the gel surface and reduce the proportion of surface hydroxyl groups.
[0026] In the seventh step, the gel is removed from the modifier or the modifier is drained, and then the gel is dried to obtain a surface-modified aerogel.
[0027] According to the present invention, the drying method includes hot air drying at normal pressure, vacuum drying, subcritical drying, supercritical drying, and closed cycle spray drying. Subcritical drying and supercritical drying have higher temperatures and lower surface tensions, and the resulting aerogel shrinkage rate is slightly lower than that of hot air drying with nitrogen gas introduced at normal pressure. Since the surface modifiers selected in the present invention have relatively high boiling points, vacuum drying is mainly used to increase the thoroughness of drying. The above-mentioned multiple drying methods are often combined to achieve the best drying effect of aerogel.
[0028] In addition, in order to reduce operating costs and surface modification efficiency, it is also necessary to increase the reuse of materials and increase the content of highly active reactants.
[0029] According to the present invention, the acid solution removed from the heating system can be used again for inorganic oxide hydrogel soaking after being dehydrated by distillation. This is because the azeotrope of hydrogen chloride and water contains 20.2wt% hydrogen chloride and the azeotropic point is 108.6°C, and this concentration of hydrochloric acid is sufficient to catalyze surface modification. In addition, the boiling points of dimethylsilanediol and tetramethyldihydroxydisiloxane, which are highly soluble in water, are also higher than the boiling point of water. Therefore, the acid solution can be completely dehydrated by distillation and then reused.
[0030] According to the present invention, before the modification liquid is used, kaolin, gibbsite, activated alumina and molecular sieve with a water content of no more than 30wt% can be soaked in it. The above materials can be used as Bronsted acid to catalyze the hydrolysis of polydimethylsilane in the presence of trace water, and finally produce dimethylsilanediol and tetramethyldihydroxydisiloxane, two substances with high solubility in water and capable of surface modification. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The hydrothermally surface modified gel can be suspended in acid solution. DETAILED DESCRIPTION
[0032] The diluted sodium water glass (modulus 3.3) is neutralized with dilute sulfuric acid to obtain silica sol, and then the silica sol is diluted with water to a silica content of about 60 g / L. The silica sol is allowed to stand for gelation and aging. The gel is then washed with deionized water until the conductivity of the washed water is less than 200 μS / cm, and a 6wt% silica hydrogel is obtained.
[0033] Example 1
[0034] Soak 6wt% silica hydrogel particles (3-5mm) in 6mol / L hydrochloric acid at room temperature for 24 hours. Then soak the acidic silica hydrogel in a container containing octamethylcyclotetrasiloxane and heat it to 60°C. Then heat it to 100°C at a rate of 10°C / hour. After keeping warm for 20 hours, drain the acid at the bottom of the container. Then continue heating and distill water at a constant rate. When no more water is distilled, heat the octamethylcyclotetrasiloxane in the container to 160°C and keep it warm for 12 hours. Empty all the octamethylcyclotetrasiloxane in the container, and then dry the silica gel with hot air at 220°C to obtain silica aerogel particles with a super-hydrophobic surface and a density of about 0.10g / cm 3 .
[0035] Comparative Example 1
[0036] Silica hydrogel particles (3-5mm) containing 6wt% were immersed in 6mol / L hydrochloric acid at room temperature for 24 hours. The acidic silica hydrogel was then immersed in a container containing octamethylcyclotetrasiloxane and heated to 60°C. After 24 hours of heat preservation, the gel was removed and dried with hot air at 220°C. The silica particles obtained at last had a large volume shrinkage rate and a density of about 0.7g / cm 3 , absorbing water. There are no drops of liquid insoluble in octamethylcyclotetrasiloxane at the bottom of the container.
[0037] Comparative Example 2
[0038] Soak 6wt% silica hydrogel particles (3-5mm) in 4mol / L hydrochloric acid at room temperature for 24 hours. Then soak the acidic silica hydrogel in a hydrothermal reaction vessel filled with octamethylcyclotetrasiloxane and heat it to 150°C. After keeping warm for 6 hours, wait for it to drop to room temperature, remove the gel, and dry it with hot air at 220°C. Finally, super-hydrophobic silica aerogel particles with a density of about 0.11g / cm 3 The liquid just taken out of the reactor has obvious stratification, and the gel is almost completely distributed in the upper liquid.
[0039] Comparative Example 3
[0040] Silica hydrogel particles (3-5 mm) containing 6 wt% were immersed in 0.1 mol / L hydrochloric acid at room temperature for 24 hours. The acidic silica hydrogel was then immersed in a container containing octamethylcyclotetrasiloxane and heated to 95°C. After 48 hours of heat preservation, the gel was removed and dried with hot air at 220°C. The silica particles obtained at last had a large volume shrinkage rate and a density of about 0.9 g / cm 3 , absorbing water. There are no drops of liquid insoluble in octamethylcyclotetrasiloxane at the bottom of the container.
[0041] Example 2
[0042] Silica hydrogel particles (3-5mm) containing 6wt% are immersed in 4mol / L hydrochloric acid at room temperature for 24 hours. Then the acidic silica hydrogel is immersed in a hydrothermal reaction container containing octamethylcyclotetrasiloxane, and the temperature is directly raised to 150°C and kept warm for 6 hours. The acid liquid at the bottom of the container is continuously discharged during the insulation process. After that, the heating and insulation are continued, and water is distilled at a constant rate. When no more water is evaporated, the octamethylcyclotetrasiloxane in the container is heated to 250°C. After the temperature is reached, all octamethylcyclotetrasiloxane in the container is emptied, and subcritical drying is performed under an absolute pressure of 5 atmospheres and 250°C. Finally, the silica gel is dried with hot air at 250°C to obtain silica aerogel particles with a surface super-hydrophobicity, with a density of about 0.10g / cm 3 The difference between the aerogel particles of Example 1 and those of Example 2 is that some of the aerogel particles of Example 2 are smaller than 0.5 mm in size, and some of them are similar in shape to those of Example 1.
[0043] Example 3
[0044] Pour the silica sol containing 6wt% silica into a 1cm thick glass fiber felt, then let it stand for gelation, aging and washing. After the composite gel is soaked in 4mol / L hydrochloric acid for 24 hours, soak the composite gel in a container containing a dimethylcyclosiloxane mixed ring body and heat it to 80℃. After keeping it warm at 80℃ for 6 hours, heat it to 150℃ at a rate of 10℃ / hour per hour and keep it warm for 3 hours. During the heating and insulation process, continuously discharge the acid liquid at the bottom of the container. Continue heating and insulation, and distill water at a constant rate. After the water is distilled, keep it warm at 150℃ for another 8 hours. Then empty the dimethylcyclosiloxane mixed ring body in the container, dry the gel with hot air at 250℃, and you can get a silica aerogel composite glass fiber felt. The surface of the fiber felt is super hydrophobic and there are no obvious cracks in the surface aerogel.
[0045] Example 4
[0046] Pour the silica sol containing 6wt% silica into a 1cm thick glass fiber felt, and then let it stand for gelation, aging and washing. After the composite gel is soaked in 3mol / L hydrochloric acid for 24 hours, soak the composite gel in a container filled with dimethyldichlorosilane hydrolyzate, heat it to 110℃ and keep it warm for 40 hours. During the heating and insulation process, continuously discharge the acid liquid at the bottom of the container. Continue heating and insulation, and distill water at a constant rate. After the water is distilled, keep it warm at 110℃ for another 8 hours. Then empty the dimethyldichlorosilane hydrolyzate in the container, vacuum dry it at 215℃ for 4 hours, and you can get a silica aerogel composite glass fiber felt. The surface of the fiber felt is super hydrophobic and there are no obvious cracks in the surface aerogel.
[0047] Example 5
[0048] After immersing a 6wt% silica gel sheet (2.5cm in diameter, 0.5cm in thickness) in 6mol / L hydrochloric acid for 24 hours, the composite gel was immersed in a container containing octamethylcyclotetrasiloxane and heated to 95°C for 48 hours. The gel did not shrink after the insulation.
[0049] Drain the acid at the bottom of the container, seal the container, and heat to 330°C. Keep it warm for 30 minutes, then start to release the pressure at a rate of 0.05 bar / minute. After the pressure is released to normal pressure, evacuate the container and cool it to room temperature. The silica aerogel taken out of the container has no shrinkage, and the surface of the aerogel is super hydrophobic, with a density of about 0.08 g / cm 3 .
[0050] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing aerogel based on hydrothermal surface modification, the method comprising the following steps: (a) firstly immersing a low-salt content inorganic oxide hydrogel in an acid solution; (b) soaking the acidic hydrogel after being soaked in the acid solution in a modifier; (c) heating the modifying agent comprising the acidic hydrogel to perform surface methylation modification; (d) During the surface methylation modification process, the acid solution must be removed from the heating system in a timely manner; (e) When the lower layer of acid is no longer noticeable, remove the residual water in the gel by distillation; (f) continuing to keep the modifier containing the gel warm; (g) After removing the gel from the modifier or draining the modifier, the gel is dried to obtain a surface-modified aerogel.
2. The method according to claim 1, wherein the inorganic oxide is amorphous silicon dioxide, titanium dioxide, zirconium dioxide, hafnium dioxide, and a combination of the above substances.
3. The method according to claim 1, wherein the hydrogel may contain silicon dioxide, titanium dioxide, silicon carbide, zirconium dioxide, aluminum oxide, graphite, carbon black powder; and aluminum silicate fiber, glass fiber, pre-oxidized fiber, high silica glass fiber, polycrystalline mullite fiber, zirconium oxide fiber, aluminum oxide fiber, polyimide fiber, polyamide fiber, polyester fiber, cellulose fiber, melamine foam.
4. according to the method for claim 1, wherein the acid solution is an aqueous solution of hydrochloric acid, hydrobromic acid, hydroiodic acid, or sulfuric acid, and the hydrogen ion concentration is greater than 1 mol / L.
5. The method according to claim 1, wherein the modifier comprises octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, hexamethyldisiloxane, octamethyltrisiloxane, a mixed ring of dimethylcyclosiloxane, a hydrolyzate of dimethyldichlorosilane, an alkane or aromatic hydrocarbon having a carbon number of 6 to 16, and a combination of the above-mentioned substances.
6. The method according to claim 1, wherein the surface methylation modification temperature is 60-150°C, preferably gradually increasing from low to high.
7. The method according to claim 1, wherein the holding temperature is 100-350°C.
8. The method according to claim 1, wherein the drying method comprises atmospheric hot air drying, vacuum drying, subcritical drying, supercritical drying, and closed cycle spray drying.
9. The method according to claim 1, wherein the acid solution removed from the heating system can be used again for soaking the inorganic oxide hydrogel after being dehydrated by distillation.
10. The method according to claim 1, wherein the modifying liquid is soaked with kaolin, gibbsite, activated alumina and molecular sieve having a water content not exceeding 30 wt% before use.