Integral CO2 adsorbent as well as preparation method and application thereof

By doping silicon carbide in calcium-based CO2 adsorbent and adopting microwave heat treatment, an integral CO2 adsorbent with high mechanical strength and adsorption capacity is formed, which solves the sintering and channel collapse of the adsorbent under high temperature conditions, and realizes the adsorbent long-term recycling and structural stability.

CN119016016AActive Publication Date: 2024-11-26CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310605022.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

The existing calcium-based CO2 adsorbents are prone to sintering, channel collapse, and adsorption capacity is reduced under high temperature conditions. The traditional high Taman temperature inert components cannot meet the mechanical strength requirements of the integrated adsorbents. The coating is not firm enough for the coating preparation. , easy to fall off.

Method used

Using the preparation method of silicon carbide-doped integrated CO2 adsorbent, the calcium-containing compound and solvent are added after drying and calcining treatment of silicon carbide precursor and additives, and heat treatment is further carried out under microwave conditions to form a polyurethane foam impregnated structure. Form an adsorbent with high mechanical strength and adsorption capacity.

Benefits of technology

The adsorbent has achieved low pressure drop, adjustable porosity, anti-sintering, high strength, and long-term recycling. The microwave absorption characteristics of the adsorbent are improved through microwave heating, solving the problems of structural stability and strength of the adsorbent.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an integral CO2 adsorbent and a preparation method and application thereof, and the preparation method comprises the following steps: (1) under a mixing condition, mixing a carbon precursor with an auxiliary agent I solution, introducing a silicon precursor, regulating the pH value of a reaction system, drying and roasting to obtain a material I; (2) uniformly mixing a calcium-containing compound, the material I and a solvent, and then introducing an auxiliary agent II to obtain slurry; and (3) adding polyurethane foam into the slurry obtained in the step (2), carrying out dipping treatment, and further carrying out heat treatment under a microwave condition, so as to obtain the integral CO2 adsorbent. The invention also provides the integral CO2 adsorbent obtained by adopting the preparation method. The integral CO2 adsorbent is low in pressure drop in use, adjustable in porosity, high in adsorption capacity, resistant to sintering, high in strength, capable of being heated by microwaves and capable of being recycled for a long time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of adsorption separation, and in particular relates to an adsorption material for adsorption separation of carbon dioxide and a preparation method thereof. Background Art

[0002] The goal of carbon neutrality requires the capture and storage of carbon dioxide gas from the flue gas or tail gas of coal-fired power plants or other industrial processes, using high-temperature solid CO 2 Adsorbents for CO in flue gas or exhaust gas 2 Direct adsorption, its operating temperature is close to the temperature of flue gas or tail gas, easy to design and operate, no high temperature gas cooling process is required, saving costs. 2 As a high-temperature solid adsorbent with fast adsorption rate and high theoretical capacity, the adsorbent has always attracted much attention.

[0003] The integral adsorbent has uniform airflow distribution and low bed pressure drop; fast heat transfer speed and small radial and axial temperature gradients; it is not easily blocked by external dust; the internal surface utilization rate is high and it is suitable for high space velocity reactions; it is easy to install and can be installed horizontally or vertically. 2 Adsorbents are used for CO in flue gas or exhaust gas 2 Capture has great advantages, but the process environment it faces is relatively complex, and the porosity and active component content of the monolithic adsorbent need to be adjustable within a large range. At the same time, researchers often use the method of doping high-Taman temperature inert components to solve the problem of calcium-based CO 2 The adsorbent is prone to sintering and fusion, pore collapse, and rapid reduction in adsorption capacity. However, the traditional high-Tarman temperature inert components have limited improvement on the strength of the adsorbent, and it is difficult to meet the mechanical strength requirements when applied to monolithic adsorbents. The coating preparation method can solve the problem of overall mechanical strength, but there is also the problem that the coating is not strong enough and is easy to fall off.

[0004] CN102500310A discloses a method for generating Al(OH) by a sol-gel method. 3 The high-temperature and highly active calcium-based CO was obtained by coating the surface of calcium citrate particles, aging, washing, drying and calcining. 2 CN102784630A discloses a calcium-based CO 2 The preparation method of the adsorbent comprises drying a mixed solution containing a calcium precursor and an inert carrier precursor by a spray dryer, and calcining to obtain the adsorbent. However, the above patent has not yet proposed a preparation method for the monolithic adsorbent, and thus cannot give full play to the unique advantages of the monolithic adsorbent. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention aims to provide a silicon carbide doped integral CO2 The adsorbent and its preparation method. The adsorbent has medium pressure reduction, adjustable porosity, high adsorption capacity, sintering resistance, high strength, microwave heating, and long-term cyclic use.

[0006] The present invention provides an integrated CO 2 The preparation method of the adsorbent comprises the following steps:

[0007] (1) under mixing conditions, a carbon precursor is mixed with an additive I solution, a silicon precursor is introduced, the pH value of the reaction system is adjusted, and material I is obtained after drying and calcining;

[0008] (2) mixing the calcium-containing compound, material I and solvent under mixing conditions, and then introducing the additive II to obtain a slurry;

[0009] (3) adding the polyurethane foam to the slurry obtained in step (2) for impregnation treatment, and further heat treating under microwave conditions to obtain a monolithic CO 2 Adsorbent.

[0010] In some specific embodiments, the monolithic CO 2 In the preparation method of the adsorbent, the carbon precursor in step (1) can be one or more of monosaccharides, disaccharides, water-soluble polysaccharides, phenolic resins, water-soluble starches, dextrins, glycerol, furfural, and furfuryl alcohol, preferably one or more of sucrose, water-soluble starch, and phenolic resins.

[0011] In some specific embodiments, the monolithic CO 2 In the preparation method of the adsorbent, the additive I solution in step (1) comprises component A and water, wherein component A is one or more of the nitrate, carbonate, phosphate, organic acid salt, and chloride of the first metal, wherein the first metal can be selected from one or more of aluminum, iron, magnesium, copper, silver, nickel, zirconium, cerium, lanthanum, yttrium, manganese, titanium, ytterbium, and neodymium; component A is further preferably selected from one or more of aluminum nitrate, iron nitrate, magnesium nitrate, copper nitrate, silver nitrate, nickel nitrate, zirconium nitrate, cerium nitrate, lanthanum nitrate, yttrium nitrate, manganese nitrate, titanium tetrachloride, ytterbium nitrate, neodymium nitrate, basic aluminum acetate, magnesium acetate, magnesium oxalate, and zirconium acetate, and is further preferably one or more of aluminum nitrate, iron nitrate, magnesium nitrate, copper nitrate, silver nitrate, nickel nitrate, and zirconium nitrate. Based on the mass of the additive I solution, the mass concentration of component A is 0.1wt% to 15wt%.

[0012] In some specific embodiments, the monolithic CO 2In the preparation method of the adsorbent, the auxiliary agent I solution in step (1) includes component B, and component B can be one or more of silicone oil, hexamethylenetetramine, formamide, N,N-dimethylformamide, and polyethylene glycol (molecular weight of 200-20000). It is further preferred that the auxiliary agent I solution also includes an organic solvent, and the organic solvent is preferably an alcohol solvent, specifically one or more of ethanol, methanol, propanol, butanol, ethylene glycol, propylene glycol, glycerol, and butanediol, and ethanol is further preferred. Based on the mass of the auxiliary agent I solution, the concentration of the organic solvent is 1wt% to 80wt%.

[0013] In some specific embodiments, the monolithic CO 2 In the preparation method of the adsorbent, the pH value of the control system in step (1) is 1 to 12, preferably 1 to 10; the pH value of the material can be adjusted by adding acid or ammonia water, and the acid can be one or more of nitric acid, hydrochloric acid, phosphoric acid, oxalic acid, and citric acid.

[0014] In some specific embodiments, the monolithic CO 2 In the preparation method of the adsorbent, the silicon precursor in step (1) can be one or more of a soluble silicate, an alkoxysilane, and silicon tetrachloride; wherein the soluble silicate can be at least one of sodium silicate, lithium silicate, potassium silicate, ammonium silicate, etc.; the alkoxysilane can be at least one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, isopropyl orthosilicate, dimethyldiethoxysilane, methyltriethoxysilane, methyltrimethoxysilane, vinyltriethoxysilane, n-octyltriethoxysilane, etc.; preferably one or more of sodium silicate, ethyl orthosilicate, and dimethyldiethoxysilane.

[0015] In some specific embodiments, the monolithic CO 2 In the preparation method of the adsorbent, based on the mass of the silicon precursor, the mass ratio of the carbon precursor to the silicon precursor is 0.3:1-10:1, the dry basis content of component A is 0.01wt%-10.0wt%, and preferably, the dry basis content of component B is 1wt%-50wt%.

[0016] In some specific embodiments, the monolithic CO 2 In the method for preparing the adsorbent, the drying temperature in step (1) is 100-150°C.

[0017] In some specific embodiments, the monolithic CO 2In the preparation method of the adsorbent, the calcination temperature in step (1) is 350-900°C, and the calcination time is 0.2-10 hours; the calcination in step (1) is carried out under an inert atmosphere and / or a reducing atmosphere, preferably under a reducing atmosphere; the inert atmosphere is nitrogen and / or an inert gas, and the inert gas is one or more of helium, neon, argon, krypton, and xenon. The reducing atmosphere is any one of a reducing gas and a mixed gas of a reducing gas and an inert atmosphere; the reducing gas is one or more of hydrogen, carbon monoxide, methane, and C2-C4 gas, preferably hydrogen and / or methane; the volume content of the reducing gas in the mixed gas is 0.5-99.5%.

[0018] In some specific embodiments, the monolithic CO 2 In the method for preparing the adsorbent, in step (1), solid-liquid separation is preferably performed before drying, and the solid phase material obtained by separation is dried.

[0019] In some specific embodiments, the monolithic CO 2 In the preparation method of the adsorbent, the calcium-containing compound in step (2) is one or more of calcium oxide, calcium hydroxide, and calcium salt. The specific calcium-containing compound can be one or more of calcium oxalate, calcium gluconate, calcium hydroxide, calcium oxide, calcium carbonate, calcium acetate, calcium propionate, calcium acetylacetonate, calcium lactate, calcium formate, calcium citrate, and calcium nitrate, and is more preferably one or more of calcium oxalate, calcium oxide, and calcium nitrate.

[0020] In some specific embodiments, the monolithic CO 2 In the preparation method of the adsorbent, the solvent in step (2) is water and / or an organic solvent, and the organic solvent is an alcohol solvent; the alcohol solvent can be specifically selected from one or more of ethanol, methanol, propanol, butanol, ethylene glycol, propylene glycol, glycerol, and butanediol, and ethanol is more preferably selected; when the solvent is a mixed solvent composed of water and an organic solvent, the concentration of the organic solvent is 1wt% to 80wt%.

[0021] In some specific embodiments, the monolithic CO 2 In the preparation method of the adsorbent, the auxiliary agent II in step (2) can be selected from one or more of carboxymethyl cellulose, hydroxyethyl cellulose, microcrystalline cellulose, chitosan, sesbania powder, hydroxypropyl methyl cellulose, polyvinyl alcohol (molecular weight 0.5 to 150,000), silica sol, aluminum dihydrogen phosphate and their solutions, preferably one or more of carboxymethyl cellulose, sesbania powder, polyvinyl alcohol (molecular weight 0.5 to 150,000), silica sol and their solutions.

[0022] In some specific embodiments, the monolithic CO2 In the preparation method of the adsorbent, in step (2), based on the mass of the calcium-containing compound, the mass ratio of the solvent to the calcium-containing compound is 2:1 to 20:1, the weight ratio of the material I to the calcium-containing compound is 0.01:1 to 2:1, and the dry basis content of the auxiliary agent II is 0.5wt% to 10wt%.

[0023] In some specific embodiments, the monolithic CO 2 In the method for preparing the adsorbent, the polyurethane foam in step (3) is a soft polyurethane foam having pores that are interconnected and have a pore size of 5 to 200 ppi (pores per inch).

[0024] In some specific embodiments, the monolithic CO 2 In the preparation method of the adsorbent, the polyurethane foam is preferably subjected to a modification treatment, and the modification treatment is to treat the polyurethane foam in an acid solution or an alkaline solution and then wash it. The acid can be one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, oxalic acid, and citric acid, and the mass concentration of the acid solution is 1wt% to 20wt%; the alkali can be one or more of sodium hydroxide, potassium hydroxide, and lithium hydroxide, and the mass concentration of the alkaline solution is 1wt% to 20wt%, and the treatment time is 1 to 10 hours. The washing is washing with deionized water, and the washing is further preferably carried out under ultrasonic conditions.

[0025] In some specific embodiments, the monolithic CO 2 In the preparation method of the adsorbent, the impregnation treatment process in step (3) is to immerse the polyurethane foam in the slurry obtained in step (2), take it out and roll it to squeeze out the excess slurry, then place it in a vacuum dryer at 60 to 150° C. and dry it for 5 to 35 minutes before taking it out. It is preferred to repeat the above process several times, such as 3 to 10 times.

[0026] In some specific embodiments, the monolithic CO 2 In the preparation method of the adsorbent, after the impregnation treatment in step (3), a calcination treatment may be optionally performed, the calcination temperature is 350 to 900° C., the calcination time is 1 to 10 hours, and the calcination is performed in the presence of an inert atmosphere, wherein the inert atmosphere is nitrogen and / or an inert gas, and the inert gas is one or more of helium, neon, argon, krypton, and xenon.

[0027] In some specific embodiments, the monolithic CO 2In the preparation method of the adsorbent, the microwave power of the heat treatment in step (3) is 10-1000 W / (g material), preferably 100-500 W / (g material); the treatment time is 0.1 to 10 hours, preferably 0.1 to 1 hour; the heat treatment is preferably carried out in the presence of an inert gas, and the inert gas is one or more of helium, neon, argon, krypton, and xenon.

[0028] In some specific embodiments, the monolithic CO 2 In the preparation method of the adsorbent, the monolithic CO 2 The preparation method of the adsorbent further comprises step (4), wherein the step (4) is to heat-treat the material obtained in step (3) under oxygen-containing atmosphere. The oxygen-containing atmosphere may be any one of air, oxygen, and a mixture of oxygen and an inert atmosphere, wherein the volume content of oxygen in the mixture is 5 to 99.99%; the inert atmosphere is nitrogen and / or an inert gas, wherein the inert gas is one or more of helium, neon, argon, krypton, and xenon. The heat treatment temperature is 500 to 1300° C., preferably 500 to 800° C., and the heat treatment time is 0.5 to 8 hours.

[0029] The second aspect of the present invention provides an integrated CO 2 The monolithic CO adsorbent 2 The adsorbent is obtained by the preparation method provided above.

[0030] Another aspect of the present invention provides the above-mentioned integral CO 2 Adsorbent and / or the integral CO prepared by the above-described method 2 The adsorbent adsorbs CO 2 Application in.

[0031] Compared with the prior art, the integrated CO 2 The adsorbent and its preparation method have the following advantages:

[0032] 1. The monolithic CO provided by the present invention 2 The adsorbent has uniform pores. Its shape and porosity can be controlled by selecting polyurethane foams of different shapes and pore sizes. It has good permeability, which is beneficial to reduce the bed pressure drop and the probability of channel flow. It is more suitable for capturing CO in flue gas or exhaust gas. 2 This high dust and high air velocity process. At the same time, the adsorbent has a three-dimensional network continuous structure that is interconnected, which is conducive to the transfer of reaction heat.

[0033] 2. The monolithic CO provided by the present invention 2In the preparation method of the adsorbent, silicon carbide is introduced through an in-situ reaction by the sol-gel method. Silicon carbide has excellent mechanical strength, thermal stability, and chemical inertness. As a supporting skeleton, it effectively prevents CaO from sintering while also providing sufficient strength to the overall adsorbent, avoiding the adsorbent from pulverizing and increasing pressure drop after multiple cycles, and ensuring long-term recycling. The supporting skeleton formed by the sol-gel method can regulate the surface morphology and pore structure of the adsorbent to a certain extent, ensuring the structure and adsorption stability of the adsorbent. At the same time, the three-dimensional network silicon carbide structure can cause microwaves to be continuously lost inside the structure, so that the adsorbent has better microwave absorption characteristics.

[0034] 3. The monolithic CO provided by the present invention 2 In the adsorbent preparation method, the use of microwaves can solve the contradiction between the high temperature of silicon carbide formation and the easy sintering of CaO active particles. In the microwave field, the dielectric properties of carbon, metal particles formed by component B, silicon carbide and calcium oxide are very different. Compared with calcium oxide, they are almost impossible to be heated. The heating rate of the first three is large, and the metal particles will produce Joule heating effect and even induce microwave discharge. This enhanced microwave hot spot effect and selective heating effect can promote the formation of silicon carbide and the formation of a supporting skeleton while preventing the sintering of CaO active particles. At the same time, the introduction of some metals in component B can also reduce the difficulty of silicon carbide synthesis or generate inert components with high Tamman temperature, further alleviating and preventing the sintering of CaO active particles. DETAILED DESCRIPTION

[0035] The specific contents and effects of the method of the present invention are further described below by way of specific examples, but the scope of the present invention is not limited thereby. In the present invention, the molecular weight of the polyvinyl alcohol is the viscosity average molecular weight.

[0036] The specific embodiments of the present invention are described in detail below, but it should be pointed out that the protection scope of the present invention is not limited by these specific embodiments, but is determined by the claims in the appendix.

[0037] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definitions in this specification shall prevail.

[0038] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.

[0039] Unless otherwise expressly indicated, throughout the specification and claims, the term "comprise" or its variations such as "include" or "comprising" etc. will be understood to include the stated elements or components without excluding other elements or other components. In this document, all numerical values ​​of parameters (e.g., quantities or conditions) are to be understood as being modified in all cases by the term "about", regardless of whether "about" actually appears before the numerical value.

[0040] Unless otherwise specified, all percentages, parts, ratios, etc. mentioned in this specification are based on weight and pressure is gauge pressure.

[0041] In the context of this specification, any two or more embodiments of the present invention may be arbitrarily combined, and the technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.

[0042] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.

[0043] Example 1

[0044] Aluminum nitrate and formamide are added to deionized water containing 40% ethanol, stirred rapidly, sucrose is added, and then tetraethyl orthosilicate is slowly added, and the pH is adjusted to 8-9 with aqueous ammonia. Wherein, based on the mass of tetraethyl orthosilicate, the aluminum nitrate content is 5%, the formamide content is 20%, and the mass ratio of sucrose to tetraethyl orthosilicate is 2:1. Dry at 120°C, and then keep constant temperature at 600°C in a hydrogen atmosphere for 2 hours to obtain material I.

[0045] Calcium nitrate is slowly added to deionized water, stirred rapidly, and then material I is slowly added, and then sesbania powder and silica sol are slowly added to obtain a slurry. Wherein, based on the mass of calcium nitrate, the mass ratio of solvent to calcium nitrate is 10:1, the weight ratio of material I to calcium nitrate is 0.2:1, the dry basis content of sesbania powder is 5%, and the dry basis content of silica sol is 0.5%.

[0046] A soft polyurethane foam with a pore size of 100 ppi (pores per inch) and interconnected pores was selected as a template, and the polyurethane foam was soaked in a 20% NaOH solution for 5 hours, and then washed with deionized water. The polyurethane foam was immersed in the slurry, and after being taken out, the excess slurry was squeezed out by rollers, and placed in a vacuum dryer to dry at 120°C, and taken out after 35 minutes. The above process was repeated 5 times, and then kept at a constant temperature of 350°C for 10 hours in a nitrogen atmosphere. The above material was sent to a microwave roasting furnace and treated at a power of 500W / (g material) for 1 hour in an argon atmosphere. The above material was kept at a constant temperature of 500°C in an air atmosphere for 4 hours to obtain an integral CO 2 Adsorbent.

[0047] Example 2

[0048] Add nickel nitrate, zirconium nitrate and N,N-dimethylformamide to deionized water containing 1% methanol, stir rapidly, add glucose, then slowly add sodium silicate, and adjust the pH to 1-2 with hydrochloric acid. Wherein, based on the mass of sodium silicate, the nickel nitrate content is 0.5%, the zirconium nitrate content is 8%, the N,N-dimethylformamide content is 50%, and the mass ratio of glucose to sodium silicate is 10:1. Dry at 150°C, and then keep constant temperature at 700°C in a hydrogen atmosphere for 7 hours to obtain material I.

[0049] Calcium oxide is slowly added to deionized water containing 5% ethanol, stirred rapidly, and then material I is slowly added, and then carboxymethyl cellulose and silica sol are slowly added to obtain a slurry. Wherein, based on the mass of calcium oxide, the mass ratio of the solvent to calcium oxide is 20:1, the weight ratio of material I to calcium oxide is 2:1, the dry basis content of carboxymethyl cellulose is 5%, and the dry basis content of silica sol is 1%.

[0050] A soft polyurethane foam with a pore size of 150 ppi (pores per inch) and interconnected pores was selected as a template, and the polyurethane foam was soaked in a 20wt% oxalic acid solution for 7 hours, and then washed with deionized water. The polyurethane foam was immersed in the slurry, and after being taken out, the excess slurry was squeezed out by roller pressing, and placed in a vacuum dryer to dry at 120°C, and taken out after 35 minutes. The above process was repeated 6 times, and then kept at a constant temperature of 600°C for 1 hour in a nitrogen atmosphere. The above material was sent to a microwave roasting furnace and treated at a power of 400W / (g material) for 1 hour in an argon atmosphere. The above material was kept at a constant temperature of 400°C in an air atmosphere for 8 hours to obtain an integral CO 2 Adsorbent.

[0051] Example 3

[0052] Zirconium nitrate is added to deionized water containing 80% methanol, stirred rapidly, phenolic resin is added, and then methyl orthosilicate is slowly added, and the pH is adjusted to 5-6 with phosphoric acid. Wherein, based on the mass of methyl orthosilicate, the content of zirconium nitrate is 4%, and the mass ratio of phenolic resin to methyl orthosilicate is 3:1. Dry at 150°C, and then keep the temperature at 800°C in a methane atmosphere for 3 hours to obtain material I.

[0053] Calcium oxalate was slowly added to deionized water containing 1% glycerol, and the mixture was stirred rapidly. Then, material I was slowly added, and then polyvinyl alcohol (average molecular weight was 22000) and aluminum dihydrogen phosphate were slowly added to obtain a slurry. The mass ratio of the solvent to calcium oxalate was 5:1, the weight ratio of material I to calcium oxalate was 0.6:1, the dry basis content of polyvinyl alcohol (average molecular weight was 22000) was 0.5%, and the dry basis content of aluminum dihydrogen phosphate was 0.5%.

[0054] A soft polyurethane foam with a pore size of 200 ppi (pores per inch) and interconnected pores was selected as a template, and the polyurethane foam was soaked in a 1% nitric acid solution for 10 hours, and then washed with deionized water. The polyurethane foam was immersed in the slurry, and after being taken out, the excess slurry was squeezed out by rollers, and placed in a vacuum dryer to dry at 140°C, and taken out after 10 minutes. The above process was repeated 7 times, and then kept at a constant temperature of 650°C for 4 hours in a nitrogen atmosphere. The above material was sent to a microwave roasting furnace and treated at a power of 1000W / (g material) for 0.5 hours in an argon atmosphere. The above material was kept at a constant temperature of 650°C for 2 hours in a nitrogen atmosphere containing 50% oxygen to obtain an integral CO 2 Adsorbent.

[0055] Example 4

[0056] Add magnesium nitrate and polyethylene glycol (molecular weight 200) to deionized water, stir rapidly, add dextrin, then slowly add potassium silicate, and adjust the pH to 2-3 with nitric acid. Wherein, based on the mass of potassium silicate, the content of magnesium nitrate is 1%, the content of polyethylene glycol (molecular weight 200) is 10%, and the mass ratio of dextrin to potassium silicate is 1.5:1. Separate the solid and liquid, dry at 120°C, and then keep constant temperature at 900°C in ethane atmosphere for 2 hours to obtain material I.

[0057] Calcium lactate was slowly added to deionized water containing 80% methanol, stirred rapidly, and then material I was slowly added, and then microcrystalline cellulose and aluminum dihydrogen phosphate were slowly added to obtain a slurry. Wherein, based on the mass of calcium lactate, the mass ratio of the solvent to calcium lactate was 2:1, the weight ratio of material I to calcium lactate was 0.1:1, the dry basis content of microcrystalline cellulose was 9%, and the dry basis content of aluminum dihydrogen phosphate was 1%.

[0058] A soft polyurethane foam with a pore size of 20 ppi (pores per inch) and interconnected pores was selected as a template, and the polyurethane foam was soaked in a 10% hydrochloric acid solution for 1 hour, and then washed with deionized water. The polyurethane foam was immersed in the slurry, and after being taken out, the excess slurry was squeezed out by rollers, and placed in a vacuum dryer to dry at 60°C, and taken out after 35 minutes. The above process was repeated 10 times, and then kept at a constant temperature of 800°C in a nitrogen atmosphere for 0.5 hour. The above material was sent to a microwave roasting furnace and treated at a power of 100W / (g material) for 1.5 hours in an argon atmosphere. The above material was kept at a constant temperature of 800°C in an oxygen atmosphere for 1 hour to obtain an integral CO 2 Adsorbent.

[0059] Comparative Example 1

[0060] Add formamide to deionized water containing 40% ethanol, stir rapidly, add sucrose, then slowly add tetraethyl orthosilicate, and adjust the pH to 8-9 with aqueous ammonia. Wherein, based on the mass of tetraethyl orthosilicate, the formamide content is 20%, and the mass ratio of sucrose to tetraethyl orthosilicate is 2:1. Dry at 120°C, and then keep constant temperature at 600°C for 2 hours in a hydrogen atmosphere to obtain material I.

[0061] Calcium nitrate is slowly added to deionized water, stirred rapidly, and then material I is slowly added, and then sesbania powder and silica sol are slowly added to obtain a slurry. Wherein, based on the mass of calcium nitrate, the mass ratio of solvent to calcium nitrate is 10:1, the weight ratio of material I to calcium nitrate is 0.2:1, the dry basis content of sesbania powder is 5%, and the dry basis content of silica sol is 0.5%.

[0062] A soft polyurethane foam with a pore size of 100 ppi (pores per inch) and interconnected pores was selected as a template, and the polyurethane foam was soaked in a 20% NaOH solution for 5 hours, and then washed with deionized water. The polyurethane foam was immersed in the slurry, and after being taken out, the excess slurry was squeezed out by rollers, and placed in a vacuum dryer to dry at 120°C, and taken out after 35 minutes. The above process was repeated 5 times, and then kept at a constant temperature of 350°C for 10 hours in a nitrogen atmosphere. The above material was sent to a microwave roasting furnace and treated at a power of 500W / (g material) for 1 hour in an argon atmosphere. The above material was kept at a constant temperature of 500°C in an air atmosphere for 4 hours to obtain an integral CO 2 Adsorbent.

[0063] Comparative Example 2

[0064] SiC micropowder, aluminum oxide, yttrium oxide and carbon black are mixed and ground to obtain material I. In which, based on the mass of SiC micropowder, aluminum oxide is 5%, yttrium oxide is 2% and carbon black is 10%.

[0065] Calcium nitrate was slowly added to deionized water, stirred rapidly, and then material I was slowly added, and then sesbania powder and silica sol were slowly added to obtain a slurry. Wherein, based on the mass of calcium nitrate, the mass ratio of solvent to calcium nitrate was 5:1, the weight ratio of material I to calcium nitrate was 0.1:1, the dry basis content of sesbania powder was 5%, and the dry basis content of silica sol was 0.5%.

[0066] A soft polyurethane foam with a pore size of 100 ppi (pores per inch) and interconnected pores was selected as a template, and the polyurethane foam was soaked in a 20% NaOH solution for 5 hours, and then washed with deionized water. The polyurethane foam was immersed in the slurry, and after being taken out, the excess slurry was squeezed out by rollers, and placed in a vacuum dryer to dry at 120°C, and taken out after 35 minutes. The above process was repeated 5 times, and then kept at a constant temperature of 350°C for 10 hours in a nitrogen atmosphere. The above material was sent to a microwave roasting furnace and treated at a power of 500W / (g material) for 3 hours in an argon atmosphere. The above material was kept at a constant temperature of 500°C in an air atmosphere for 4 hours to obtain an integral CO 2 Adsorbent.

[0067] Comparative Example 3

[0068] Aluminum nitrate and formamide are added to deionized water containing 40% ethanol, stirred rapidly, sucrose is added, and then tetraethyl orthosilicate is slowly added, and the pH is adjusted to 8-9 with aqueous ammonia. Wherein, based on the mass of tetraethyl orthosilicate, the aluminum nitrate content is 5%, the formamide content is 20%, and the mass ratio of sucrose to tetraethyl orthosilicate is 2:1. Dry at 120°C, and then keep constant temperature at 600°C in a hydrogen atmosphere for 2 hours to obtain material I.

[0069] Calcium nitrate is slowly added to deionized water, stirred rapidly, and then material I is slowly added, and then sesbania powder and silica sol are slowly added to obtain a slurry. Wherein, based on the mass of calcium nitrate, the mass ratio of solvent to calcium nitrate is 10:1, the weight ratio of material I to calcium nitrate is 0.2:1, the dry basis content of sesbania powder is 5%, and the dry basis content of silica sol is 0.5%.

[0070] A soft polyurethane foam with a pore size of 100 ppi (pores per inch) and interpenetrating pores was selected as a template, and the polyurethane foam was soaked in a 20% NaOH solution for 5 hours, and then washed with deionized water. The polyurethane foam was immersed in the slurry, taken out and rolled to squeeze out the excess slurry, placed in a vacuum dryer at 120°C and dried, and taken out after 35 minutes. The above process was repeated 5 times, and then kept at a constant temperature of 1700°C for 7 hours in an argon atmosphere. The above material was kept at a constant temperature of 500°C in an air atmosphere for 4 hours to obtain a monolithic CO 2 Adsorbent.

[0071] Adsorbent performance evaluation:

[0072] The monolithic CO was prepared by Examples 1-4 and Comparative Examples 1-3. 2 CO of adsorbent 2 The adsorption capacity was measured by thermogravimetric analyzer (TGA) under the following conditions: adsorption temperature was 650°C, desorption temperature was 800°C, the number of cycles was 100, and the average value was taken. The results are shown in Table 1:

[0073] Table 1 CO of adsorbent 2 Adsorption capacity

[0074] catalyst <![CDATA[Adsorption capacity / g CO2 / g 吸附剂 > Example 1 0.43 Example 2 0.37 Example 3 0.40 Example 4 0.42 Comparative Example 1 0.33 Comparative Example 2 0.13 Comparative Example 3 0.03

Claims

1. A method for preparing a monolithic CO2 adsorbent, comprising the following steps: (1) Under mixing conditions, a carbon precursor is mixed with an additive I solution, a silicon precursor is introduced, the pH value of the reaction system is adjusted, and material I is obtained after drying and calcination; the additive I solution includes component A and water, wherein component A is one or more of a nitrate, carbonate, phosphate, organic acid salt, and chloride of a first metal, wherein: The first metal is selected from one or more of aluminum, iron, magnesium, copper, silver, nickel, zirconium, cerium, lanthanum, yttrium, manganese, titanium, ytterbium, and neodymium; (2) under mixing conditions, the calcium-containing compound, material I and solvent are mixed uniformly, and then an additive II is introduced to obtain a slurry; the additive II is selected from one or more of carboxymethyl cellulose, hydroxyethyl cellulose, microcrystalline cellulose, chitosan, sesbania powder, hydroxypropyl methyl cellulose, polyvinyl alcohol, silica sol, aluminum dihydrogen phosphate and solutions thereof; (3) Adding polyurethane foam to the slurry obtained in step (2) for impregnation treatment, and further heat-treating it under microwave conditions to obtain a monolithic CO2 adsorbent.

2. The method for preparing the integral CO2 adsorbent according to claim 1, wherein: The carbon precursor in step (1) is one or more of monosaccharide, disaccharide, water-soluble polysaccharide, phenolic resin, water-soluble starch, dextrin, glycerol, furfural, furfuryl alcohol, preferably one or more of sucrose, water-soluble starch, phenolic resin.

3. The method for preparing the integral CO2 adsorbent according to claim 1, wherein: Component A is selected from one or more of aluminum nitrate, iron nitrate, magnesium nitrate, copper nitrate, silver nitrate, nickel nitrate, zirconium nitrate, cerium nitrate, lanthanum nitrate, yttrium nitrate, manganese nitrate, titanium tetrachloride, ytterbium nitrate, neodymium nitrate, basic aluminum acetate, magnesium acetate, magnesium oxalate, and zirconium acetate, preferably one or more of aluminum nitrate, iron nitrate, magnesium nitrate, copper nitrate, silver nitrate, nickel nitrate, and zirconium nitrate.

4. The method for preparing the integral CO2 adsorbent according to claim 1, wherein: The auxiliary agent I solution includes component B, and component B is one or more of silicone oil, hexamethylenetetramine, formamide, N,N-dimethylformamide, and polyethylene glycol.

5. The method for preparing the integral CO2 adsorbent according to claim 1, wherein: The auxiliary agent I solution includes an organic solvent, and the organic solvent is an alcohol solvent.

6. The method for preparing the integral CO2 adsorbent according to claim 5, wherein: The alcohol solvent is one or more of ethanol, methanol, propanol, butanol, ethylene glycol, propylene glycol, glycerol, and butanediol, preferably ethanol.

7. The method for preparing the integral CO2 adsorbent according to claim 1, wherein: The pH value of the regulating system in step (1) is 1 to 12, preferably 1 to 10; the pH value of the material is adjusted by adding acid or ammonia water, and the acid is one or more of nitric acid, hydrochloric acid, phosphoric acid, oxalic acid, and citric acid.

8. The method for preparing the integral CO2 adsorbent according to claim 1, wherein: The silicon precursor in step (1) is one or more of a soluble silicate, an alkoxysilane, and silicon tetrachloride; wherein the soluble silicate is at least one of sodium silicate, lithium silicate, potassium silicate, and ammonium silicate; the alkoxysilane is at least one of methyl orthosilicate, ethyl orthosilicate, propyl orthosilicate, isopropyl orthosilicate, dimethyldiethoxysilane, methyltriethoxysilane, methyltrimethoxysilane, vinyltriethoxysilane, and n-octyltriethoxysilane; preferably, it is one or more of sodium silicate, ethyl orthosilicate, and dimethyldiethoxysilane.

9. The method for preparing the integral CO2 adsorbent according to claim 1, wherein: Based on the mass of the silicon precursor, the mass ratio of the carbon precursor to the silicon precursor is 0.3:1-10:1, the dry basis content of component A is 1wt%-50wt%, and the dry basis content of component B is 0.01wt%-10.0wt%.

10. The method for preparing the integral CO2 adsorbent according to claim 1, wherein: The drying temperature in step (1) is 100-150°C.

11. The method for preparing a monolithic CO2 adsorbent according to claim 1, wherein: The calcination temperature in step (1) is 350-900° C., and the calcination time is 0.2-10 hours. The calcination in step (1) is carried out under an inert atmosphere and / or a reducing atmosphere. The reducing atmosphere is any one of a reducing gas and a mixed gas of a reducing gas and an inert atmosphere, wherein the volume content of the reducing gas in the mixed gas is 0.5-99.5%. The reducing gas is one or more of hydrogen, carbon monoxide, methane, and C2-C4 gas, preferably hydrogen and / or methane. The inert atmosphere is nitrogen and / or an inert gas.

12. The method for preparing the integral CO2 adsorbent according to claim 1, wherein: The calcium-containing compound in step (2) is one or more of calcium oxide, calcium hydroxide, and calcium salt.

13. The method for preparing a monolithic CO2 adsorbent according to claim 1 or 13, wherein: The calcium-containing compound in step (2) is one or more of calcium oxalate, calcium gluconate, calcium hydroxide, calcium oxide, calcium carbonate, calcium acetate, calcium propionate, calcium acetylacetonate, calcium lactate, calcium formate, calcium citrate, and calcium nitrate, preferably one or more of calcium oxalate, calcium oxide, and calcium nitrate.

14. The method for preparing a monolithic CO2 adsorbent according to claim 1, wherein: The solvent in step (2) is water and / or an organic solvent, and the organic solvent is an alcohol solvent; the alcohol solvent is selected from one or more of ethanol, methanol, propanol, butanol, ethylene glycol, propylene glycol, glycerol, and butanediol, preferably ethanol; when the solvent is a mixed solvent composed of water and an organic solvent, the concentration of the organic solvent is 1wt% to 80wt%.

15. The method for preparing a monolithic CO2 adsorbent according to claim 1, wherein: The auxiliary agent II in step (2) is selected from one or more of carboxymethyl cellulose, sesbania powder, polyvinyl alcohol (molecular weight 0.5-150,000), silica sol and solutions thereof.

16. The method for preparing a monolithic CO2 adsorbent according to claim 1, wherein: In step (2), based on the mass of the calcium-containing compound, the mass ratio of the solvent to the calcium-containing compound is 2:1 to 20:1, the weight ratio of the material I to the calcium-containing compound is 0.01:1 to 2:1, and the dry basis content of the auxiliary agent II is 0.5wt% to 10wt%.

17. The method for preparing a monolithic CO2 adsorbent according to claim 1, wherein: The polyurethane foam in step (3) is a soft polyurethane foam having pores that are interconnected and have a pore size of 5 to 200 ppi.

18. The method for preparing a monolithic CO2 adsorbent according to claim 1 or 18, wherein: The polyurethane foam is subjected to modification treatment, which is to treat the polyurethane foam in an acid solution or an alkaline solution and then wash it to obtain the polyurethane foam; the acid is one or more of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, oxalic acid and citric acid, and the mass concentration of the acid solution is 1wt% to 20wt%; the alkali is one or more of sodium hydroxide, potassium hydroxide and lithium hydroxide, and the mass concentration of the alkaline solution is 1wt% to 20wt%, and the treatment time is 1 to 10 hours; washing is washing with deionized water, and washing is preferably carried out under ultrasonic conditions.

19. The method for preparing a monolithic CO2 adsorbent according to claim 1, wherein: After the impregnation treatment in step (3), a calcination treatment is optionally performed. The calcination temperature is 350 to 900° C., the calcination time is 1 to 10 hours, and the calcination is performed in the presence of an inert atmosphere, which is nitrogen and / or an inert gas.

20. The method for preparing a monolithic CO2 adsorbent according to claim 1, wherein: The microwave power of the heat treatment in step (3) is 10-1000 W / (g material), preferably 100-500 W / (g material); the treatment time is 0.1 to 10 hours, preferably 0.1 to 1 hour; the heat treatment is carried out in the presence of an inert gas.

21. The method for preparing a monolithic CO2 adsorbent according to claim 1, wherein: The preparation method of the integral CO2 adsorbent also includes step (4), wherein the step (4) is to heat treat the material obtained in step (3) under oxygen-containing atmosphere conditions; the heat treatment temperature is 500 to 1300°C, preferably 500 to 800°C, and the heat treatment time is 0.5 to 8 hours.

22. An integral CO2 adsorbent, wherein the integral CO2 adsorbent is obtained by the preparation method described in any one of claims 1 to 21.

23. Use of the integral CO2 adsorbent according to claim 22 and / or the integral CO2 adsorbent obtained by the preparation method according to any one of claims 1 to 22 in adsorbing CO2.

Citation Information

Patent Citations

  • Aerogel composite material with surface subjected to dust-free treatment and preparation method

    CN106007635A

  • Method for preparing high-purity hydrogen from biomass and system adopted by method

    CN111498806A

  • Catalyst carrier for tar cracking, catalyst and preparation method of catalyst carrier

    CN113117715A

  • Carrier and catalyst for integral tar cracking and preparation method of carrier and catalyst

    CN114471648A

  • Liquid curable composition

    KR1020130048748A