Carbon quantum dot modified micron-sized iron-copper bimetallic material as well as preparation method and application thereof
By modifying carbon quantum dots and nanocopper particles on the surface of Fe0 material, the electron utilization efficiency and pH application scope of Fe0 are improved, and the problem of low degradation efficiency of Fe0 material in Fenton oxidation technology is solved, and efficient degradation of organic pollutants is achieved. Bacterial disinfection reduces treatment costs.
Patent Information
- Application Number
- CN202410991774.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-26
Smart Images

Figure HDA0004959065630000011 
Figure HDA0004959065630000021 
Figure HDA0004959065630000022
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of functional materials for water treatment, and relates to a carbon quantum dot-modified micron-sized iron-copper bimetallic material, and a preparation method and application thereof. Background Art
[0002] The excessive use of antibiotics has aroused global concern about the environmental pollution caused by antibiotic residues. At present, many methods including adsorption, biological treatment, membrane treatment and advanced oxidation processes (AOPs) have been used to eliminate antibiotics in water bodies. However, the adsorption method can only separate antibiotics from the water body, but cannot degrade the antibiotics. Due to the biological resistance of antibiotics, the removal efficiency of antibiotics by biological treatment is poor. The membrane treatment method consumes a lot of energy due to its high operating pressure. In contrast, AOPs use active species such as free radicals for strong oxidation and have shown a high removal ability for a variety of organic pollutants. Among AOPs, the Fenton oxidation method has been widely used in the degradation of antibiotic organic pollutants such as sulfamethoxazole (SMX). The Fenton oxidation process produces hydroxyl radicals ( · OH), · OH can non-selectively attack a variety of organic pollutants. However, the application of the traditional Fenton oxidation method is limited by its narrow pH range, and is only applicable to wastewater treatment with a pH value of 2.8 to 3.5. At the same time, the application of the traditional Fenton oxidation method is also limited by the slow Fe(III) / Fe(II) cycle rate. Currently, an important research direction of Fenton oxidation technology is to develop catalytic materials that can promote the Fe(III) / Fe(II) cycle.
[0003] Zero valent iron (Fe 0 ) has the advantages of being eco-friendly and inexpensive. When used in water treatment, it can generate Fe(Ⅱ) in situ and combine with H2O2 to form Fenton oxidation, which has a high pollutant removal efficiency and has been widely used to remove pollutants in water. However, in actual application, due to the 0 The surface is prone to produce iron oxides and hydroxides, forming a passivation layer on its surface, resulting in Fe 0 The activity of Fe 0 Therefore, it is necessary to 0 The material is improved to improve the Fe(Ⅲ) / Fe(Ⅱ) cycle efficiency in application, broaden its pH application range, and improve the Fe-based 0 The degradation efficiency of organic pollutants by advanced oxidation process.
[0004] Currently, Fe 0The research on modification mainly focuses on modifying the surface of iron with metals such as copper, manganese, and silver, or modifying non-metals such as carbon and sulfur to form iron-based modified materials to promote Fe 0 Release electrons and release iron ions. However, most of the iron-based modified materials obtained by these modification methods are formed by two-electron reactions with strong oxidizing ability. · OH to degrade pollutants non-selectively. Few materials can generate superoxide radicals (O2 ·- ), and O2 ·- It has the ability to selectively degrade pollutants and also has good bactericidal properties. Therefore, if the existing iron-based modified materials can be improved, the electron utilization efficiency of the iron-based materials in the reaction with O2 can be improved, and O2 can be generated mainly through single-electron reactions during the wastewater treatment process. ·- To degrade pollutants, it will have a positive impact on improving the degradation effect of organic pollutants. Summary of the Invention
[0005] For existing Fe-based 0 The Fenton oxidation technique in the presence of Fe 0 The pH application range of the material is narrow, the Fe(III) / Fe(II) cycle rate is slow, the electron utilization efficiency is low, and the degradation efficiency of pollutants needs to be improved. The present invention provides a carbon quantum dot modified iron-copper bimetallic material and its preparation method and application to improve the existing Fe 0 The Fe(Ⅲ) / Fe(Ⅱ) cycle efficiency and electron utilization efficiency of the material when used in advanced oxidation processes are improved, and its pH application range is broadened to improve the degradation efficiency of organic pollutants.
[0006] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is as follows:
[0007] A carbon quantum dot-modified micron-sized iron-copper bimetallic material comprises micron-sized zero-valent iron and carbon quantum dots and nano-copper particles loaded on the surface of the micron-sized zero-valent iron. The carbon quantum dots and nano-copper particles are evenly and discretely distributed on the surface of the micron-sized zero-valent iron.
[0008] In the above-mentioned technical solution of carbon quantum dots modified micron-sized iron-copper bimetallic material, the particle size of the micron-sized zero-valent iron is preferably 40 to 120 μm.
[0009] The present invention also provides a method for preparing the carbon quantum dot-modified micron-sized iron-copper bimetallic material, comprising the following steps:
[0010] (1) adding micron-sized zero-valent iron and carbon quantum dots into a ball mill, controlling the amount of carbon quantum dots added to be 0.2 wt% to 0.8 wt% of the micron-sized zero-valent iron, and adding grinding balls into the ball mill to fully ball mill to obtain carbon quantum dot-modified micron-sized zero-valent iron;
[0011] (2) Adding the micron-sized zero-valent iron modified with carbon quantum dots to an aqueous solution of a divalent copper salt having a copper ion concentration of 2 to 20 mmol / L, controlling the amount of the added micron-sized zero-valent iron modified with carbon quantum dots so that the mass ratio of copper to zero-valent iron is 1:(5 to 10), performing a replacement reaction under stirring conditions, forming nano-copper particles on the surface of the micron-sized zero-valent iron modified with carbon quantum dots, performing solid-liquid separation, and washing the obtained solid phase with water to obtain a micron-sized iron-copper bimetallic material modified with carbon quantum dots.
[0012] In step (1) of the technical solution of the above-mentioned preparation method, a feasible method for preparing carbon quantum dots is: dissolving a carbon source in water to form a carbon source solution with a concentration of 5 to 40 g / L, adjusting the pH value of the carbon source solution to 6 to 6.5 to obtain a precursor solution; transferring the precursor solution to a high-pressure reactor, reacting at 200 to 220° C. for 4 to 6 hours to obtain a reaction solution, filtering the reaction solution with a microporous filter membrane and dialyzing it with water for 2 to 3 days, and freeze-drying the dialyzed reaction solution to obtain the product.
[0013] Furthermore, in the technical solution of the above preparation method, the carbon source is citric acid, glucose or glutamic acid.
[0014] In step (1) of the technical solution of the above preparation method, ball milling is preferably carried out at a rotation speed of 100 to 300 rpm for 15 to 60 minutes.
[0015] In step (1) of the technical solution of the above preparation method, the amount of carbon quantum dots added is preferably controlled to be 0.5 wt% to 0.8 wt% of the micron-sized zero-valent iron.
[0016] In step (2) of the technical solution of the above preparation method, the time for the replacement reaction under stirring conditions is preferably 2 to 5 minutes.
[0017] The present invention also provides the use of the carbon quantum dot-modified micron-sized iron-copper bimetallic material in treating organic wastewater.
[0018] Furthermore, when the above-mentioned carbon quantum dot-modified micron-sized iron-copper bimetallic material is used to treat organic wastewater, the above-mentioned carbon quantum dot-modified micron-sized iron-copper bimetallic material is added to the wastewater containing organic pollutants, the pH value of the wastewater is controlled to be 3-5, and the concentration of the carbon quantum dot-modified micron-sized iron-copper bimetallic material in the wastewater is controlled to be 1-100 mg / L. The wastewater is treated under stirring conditions. The carbon quantum dot-modified micron-sized iron-copper bimetallic material produces superoxide radicals and hydrogen radicals during the wastewater treatment process to achieve the degradation of organic pollutants in the wastewater.
[0019] When the above-mentioned carbon quantum dot-modified micron-sized iron-copper bimetallic material is used to treat organic wastewater, when the wastewater containing organic pollutants contains bacteria, the degradation of organic pollutants and the elimination of bacteria can be achieved simultaneously during the wastewater treatment process.
[0020] When the carbon quantum dot-modified micron-sized iron-copper bimetallic material is used to treat organic wastewater, the wastewater treatment time is determined based on the water quality of the organic wastewater. For example, the wastewater treatment time is typically determined based on the type and concentration of the organic pollutants in the wastewater. Treatment is typically performed until the removal rate of the organic pollutants in the wastewater reaches equilibrium. Generally, the wastewater treatment time does not exceed 60 minutes, and for example, the wastewater treatment time can be controlled to be 30 to 60 minutes.
[0021] When the carbon quantum dot-modified micron-sized iron-copper bimetallic material is used to treat organic wastewater, the organic pollutants in the wastewater containing organic pollutants may be antibiotics, such as sulfamethoxazole.
[0022] The main principles of the present invention are as follows:
[0023] The present invention modifies the surface of micron-sized zero-valent iron with carbon quantum dots and nano-copper particles, which are evenly and discretely distributed on the surface of micron-sized zero-valent iron. By introducing nano-copper particles for modification, the zero-valent iron can be promoted to release electrons. By introducing carbon quantum dots for modification, the adsorption and binding ability of zero-valent iron to O2 in water can be improved, which is conducive to promoting molecular oxygen to obtain an electron to generate superoxide radicals (O2 ·- ), improving the electron utilization efficiency of zero-valent iron. Furthermore, the carbon quantum dot-modified micron-sized iron-copper bimetallic material described herein can generate hydrogen free radicals during wastewater treatment. The combined action of superoxide free radicals and hydrogen free radicals effectively improves the degradation efficiency of organic pollutants.
[0024] Compared with the prior art, the technical solution provided by the present invention produces the following beneficial technical effects:
[0025] 1. The present invention provides a carbon quantum dot modified micron-sized iron-copper bimetallic material, which is composed of micron-sized zero-valent iron and carbon quantum dots and nano-copper particles loaded on the surface of the micron-sized zero-valent iron. The carbon quantum dots and nano-copper particles are evenly and discretely distributed on the surface of the micron-sized zero-valent iron. The present invention can promote the release of electrons from the zero-valent iron by introducing nano-copper particles to modify the zero-valent iron. By introducing carbon quantum dots to modify the zero-valent iron, the adsorption and binding ability of the zero-valent iron to O2 in water can be improved, which is conducive to promoting the generation of superoxide radicals (O2) by molecular oxygen gaining an electron. ·- ), improving the electron utilization efficiency of zero-valent iron. Furthermore, this carbon quantum dot-modified micron-sized iron-copper bimetallic material can also generate hydrogen free radicals during wastewater treatment. Compared to existing Fenton oxidation technology, this invention effectively improves the degradation efficiency of organic pollutants through the combined action of superoxide free radicals and hydrogen free radicals.
[0026] 2. The present invention has experimentally demonstrated that the carbon quantum dot-modified micron-sized iron-copper bimetallic material provided by the present invention, when used for wastewater treatment, can not only be used to degrade refractory organic matter, such as sulfamethoxazole, but can also effectively inhibit the growth and reproduction of bacteria, such as Escherichia coli, thereby being used to simultaneously degrade organic pollutants and disinfect bacteria. In practical applications, it can be used to degrade hospital wastewater containing both organic pollutants (such as antibiotics) and bacteria.
[0027] 3. Experiments have demonstrated that the carbon quantum dot-modified micron-sized iron-copper bimetallic material provided by the present invention can expand the pH range applicable to wastewater using existing Fenton oxidation technology from 2.8 to 3.5 to a pH range of 3 to 5. This expanded pH range not only broadens the method's applicability but also reduces the use of acid and base conditioning agents, thereby lowering wastewater treatment costs.
[0028] 4. The present invention has experimentally confirmed that when the carbon quantum dot-modified micron-sized iron-copper bimetallic material provided by the present invention is used for wastewater treatment, the degradation efficiency of organic pollutants represented by sulfamethoxazole is significantly improved compared with existing zero-valent iron and iron-copper bimetallic materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Figures (a1) and (a2) are scanning electron microscope (SEM) and energy dispersive spectrum (EDS) images of micron-scale zero-valent iron. Figure 1 Figures (b1) and (b2) are SEM and EDS images of the micron-sized iron-copper bimetallic material prepared in Comparative Example 1. Figure 1 Figures (c1) and (c2) are the SEM and EDS images of 0.5% C@mFe / nCu.
[0030] Figure 2 1 is the curve showing the change of C / C0 of SMX with reaction time in Example 2.
[0031] Figure 3 These are the XPS spectra of Fe in mFe, mFe / nCu, and 0.5% C@mFe / nCu before and after using them in SMX wastewater treatment.
[0032] Figure 4 This is the change in the number of Escherichia coli with sterilization time in Example 3.
[0033] Figure 5 4 is the curve showing the change of C / C0 of SMX over the reaction time.
[0034] Figure 6 5 is the curve showing the change of C / C0 of SMX over the reaction time.
[0035] Figure 7 This is the removal rate of SMX in SMX wastewater with different initial pH values by 0.5% C@mFe / nCu in Example 6.
[0036] Figure 8 This is the EPR test result in Example 7.
[0037] Figure 9 These are the test results of the effects of different anions on the degradation performance of SMX in Example 8. DETAILED DESCRIPTION
[0038] The following examples further illustrate the carbon quantum dot-modified micron-sized iron-copper bimetallic material provided by the present invention, its preparation method, and its application. It is important to note that the following examples are intended only to further illustrate the present invention and are not to be construed as limiting the scope of protection of the present invention. Non-essential improvements and adjustments made by persons skilled in the art to the present invention based on the above-described disclosure and implemented in a specific manner are still within the scope of protection of the present invention.
[0039] Example 1
[0040] In this embodiment, the steps for preparing a carbon quantum dot modified micron-sized iron-copper bimetallic material are as follows:
[0041] (1) Synthesis of carbon quantum dots
[0042] Citric acid was used as the carbon source. The citric acid was added to deionized water and stirred thoroughly at room temperature until dissolved to obtain a citric acid solution with a concentration of 40 g / L. Ammonia water was then added to adjust the pH value of the citric acid solution to 6. Stirring was continued for 30 minutes to obtain a precursor solution. The precursor solution was transferred to a high-pressure reactor and reacted at 200°C for 4 hours to obtain a dark green reaction solution. The obtained reaction solution was filtered with a 0.22 μm microporous membrane and dialyzed with a 500 MW dialysis bag for 2 days. The dialyzed reaction solution was freeze-dried to obtain carbon quantum dots.
[0043] (2) Preparation of micron-sized zero-valent iron modified with carbon quantum dots
[0044] Add micron-sized zero-valent iron with an average particle size of 80 μm and the carbon quantum dots prepared in step (1) into a ball mill, add zirconium oxide grinding balls into the ball mill, and ball mill at a speed of 300 rpm for 30 minutes to obtain micron-sized zero-valent iron modified with carbon quantum dots;
[0045] In this step, a total of three groups of experiments were conducted. In all three groups of experiments, the mass ratio of the sum of the mass of micron-sized zero-valent iron and carbon quantum dots to the mass of zirconia grinding balls was controlled to be 1:5, and the added amount of carbon quantum dots was controlled to be 0.2wt%, 0.5wt% and 0.8wt% of the micron-sized zero-valent iron, respectively.
[0046] (3) Copper loading on the surface of micron-sized zero-valent iron modified with carbon quantum dots
[0047] Copper sulfate pentahydrate was used as a copper source. The copper sulfate pentahydrate was added to deionized water and stirred at room temperature until dissolved to obtain a copper sulfate solution with a concentration of 7.8 mmol / L. The carbon quantum dot-modified micron-sized zero-valent iron prepared in step (2) was added thereto. The mixture was stirred at room temperature at a speed of 300 rpm for 2 min to perform a replacement reaction. The solid-liquid separation was performed, and the obtained solid phase was washed with deionized water to obtain a carbon quantum dot-modified micron-sized iron-copper bimetallic material.
[0048] In this step, a total of 12 groups of experiments were conducted, as follows:
[0049] In the first to fourth groups of experiments, the carbon quantum dot-modified micron-sized zero-valent iron prepared in step (2) was used as the basis when the amount of carbon quantum dots added was 0.2 wt % of the micron-sized zero-valent iron. The amount of carbon quantum dot-modified micron-sized zero-valent iron added was controlled so that the mass ratio of copper to zero-valent iron was 1:5, 1:10, 1:20, and 1:30, respectively.
[0050] In experiments 5 to 8, based on the carbon quantum dot-modified micron-sized zero-valent iron prepared when the amount of carbon quantum dots added in step (2) was 0.5 wt % of the micron-sized zero-valent iron, the amount of carbon quantum dot-modified micron-sized zero-valent iron added was controlled so that the mass ratio of copper to zero-valent iron was 1:5, 1:10, 1:20, and 1:30, respectively;
[0051] In groups 9 to 12 of experiments, based on the carbon quantum dot-modified micron-sized zero-valent iron prepared when the amount of carbon quantum dots added in step (2) was 0.8 wt% of the micron-sized zero-valent iron, the amount of carbon quantum dot-modified micron-sized zero-valent iron added was controlled so that the mass ratio of copper to zero-valent iron was 1:5, 1:10, 1:20, and 1:30, respectively.
[0052] Comparative Example 1
[0053] In this comparative example, the steps for preparing a micron-sized iron-copper bimetallic material are as follows:
[0054] Copper sulfate pentahydrate was used as a copper source. Copper sulfate pentahydrate was added to deionized water and stirred thoroughly at room temperature until dissolved to obtain a copper sulfate solution with a concentration of 7.8 mmol / L. Micron-sized zero-valent iron with an average particle size of 80 μm was added. The amount of micron-sized zero-valent iron added was controlled so that the mass ratio of copper to iron was 1:10. The mixture was stirred at 300 rpm at room temperature for 2 minutes to perform a replacement reaction to obtain a micron-sized iron-copper bimetallic material.
[0055] Figure 1 Figures (a1) and (a2) are scanning electron microscope (SEM) images and energy dispersive spectrum (EDS) images of micron-sized zero-valent iron (mFe for short). Figure 1 Figures (b1) and (b2) are SEM images and EDS images of the micron-sized iron-copper bimetallic material (abbreviated as mFe / nCu) prepared in comparative example 1. Figure 1 Figures (c1) and (c2) are SEM images and EDS images of a carbon quantum dot-modified micron-sized iron-copper bimetallic material (abbreviated as 0.5% C@mFe / nCu) prepared by controlling the amount of carbon quantum dot-modified micron-sized zero-valent iron added to make the mass ratio of copper to zero-valent iron 1:10, based on the carbon quantum dot-modified micron-sized zero-valent iron prepared in step (2) of Example 1. Figure 1 As shown in Figures (b1) and (b2), in the micron-sized iron-copper bimetallic material prepared in Comparative Example 1, nano-copper particles are discretely distributed on the surface of micron-sized zero-valent iron. Figure 1 As can be seen from Figures (c1) and (c2), Example 1 successfully loaded carbon quantum dots and nano-copper particles on the surface of micron-sized zero-valent iron, and the carbon quantum dots and nano-copper particles were discretely distributed on the surface of micron-sized zero-valent iron.
[0056] Example 2
[0057] In this embodiment, the degradation performance of sulfamethoxazole (SMX) on the micron-sized zero-valent iron (mFe for short) used in Example 1, the micron-sized iron-copper bimetallic material (mFe / nCu for short) prepared in Comparative Example 1, and the carbon quantum dot-modified micron-sized zero-valent iron prepared in step (2) in Example 1 when the amount of carbon quantum dots added was 0.5 wt % of the micron-sized zero-valent iron (0.5% C@mFe / nCu for short) was tested.
[0058] (1) SMX was dissolved in deionized water and the pH value was adjusted to 3 to obtain SMX wastewater with an SMX concentration of 10 μmol / L.
[0059] (2) Take three portions of SMX wastewater, add mFe, mFe / nCu, and 0.5% C@mFe / nCu to each portion of SMX wastewater, respectively, and control the concentration of mFe, mFe / nCu, and 0.5% C@mFe / nCu in each portion of SMX wastewater to be 1 mg / mL. Stir and treat the wastewater at 30°C and 300 rpm for 30 minutes. During the wastewater treatment process, samples were taken every 5 to 10 minutes and filtered with a 0.22 μm filter membrane. The concentration of SMX was determined by high performance liquid chromatography (HPLC). The ratio of the final concentration C of SMX to its initial concentration C0, C / C0, was calculated, and a curve of the change of SMX C / C0 with reaction time was plotted.
[0060] In this embodiment, when mFe or mFe / nCu or 0.5% C@mFe / nCu is added, the C / C0 curve of SMX changes with reaction time (i.e., the degradation curve of SMX) is as follows: Figure 2 As shown by Figure 2 It can be seen that under the same dosage and water quality conditions, the degradation efficiency of SMX by 0.5% C@mFe / nCu is significantly higher.
[0061] In this example, the XPS spectra of Fe in mFe, mFe / nCu, and 0.5% C@mFe / nCu were tested before and after treatment of SMX wastewater. The results are as follows: Figure 3 As shown, Figure 3 The mFe, mFe / nCu and 0.5%C@mFe / nCu in the table represent mFe, mFe / nCu and 0.5%C@mFe / nCu respectively. Figure 3 It can be seen that the Fe(III) / Fe(II) cycle rate of 0.5% C@mFe / nCu is faster and the Fe(II) regeneration ability is stronger, which means that 0.5% C@mFe / nCu has better self-renewal performance.
[0062] Example 3
[0063] In this embodiment, the micron-sized zero-valent iron (mFe for short) used in Example 1, the micron-sized iron-copper bimetallic material (mFe / nCu for short) prepared in Comparative Example 1, and the carbon quantum dot-modified micron-sized zero-valent iron prepared in step (3) of Example 1 with the amount of carbon quantum dots added in step (2) being 0.5 wt% of the micron-sized zero-valent iron as the basis were tested, and the carbon quantum dot-modified micron-sized iron-copper bimetallic material (0.5% C@mFe / nCu for short) prepared by controlling the amount of carbon quantum dot-modified micron-sized zero-valent iron added so that the mass ratio of copper to iron was 1:10 was tested for their sterilization performance against Escherichia coli.
[0064] This example includes 1 blank control group and 3 experimental groups, as follows:
[0065] Blank control group: Add 30 mL of 0.9% saline to the Erlenmeyer flask reaction vessel, adjust the pH to 7, then add 1 mL of E. coli culture solution and 1 g of zirconium oxide balls. Place the Erlenmeyer flask on a shaker and incubate at 37°C and 200 rpm for 30 minutes. During the reaction, sample 50 μL of the reaction solution every 10 minutes to determine the number of E. coli colonies.
[0066] Experimental Groups 1-3: Prepare three Erlenmeyer flasks. Add 30 mL of 0.9% saline to each flask, adjust the pH to 7, then add 1 mL of E. coli culture solution and 1 g of zirconium oxide balls, followed by 0.015 g of mFe, 0.015 g of mFe / nCu, and 0.015 g of 0.5% C@mFe / nCu, respectively. Place each flask on a shaker and incubate at 37°C and 200 rpm for 30 minutes. Every 10 minutes, sample 50 μL of the reaction solution for E. coli colony count.
[0067] The method for determining the number of Escherichia coli (i.e., colony count) is as follows: 50 μL of the reaction solution was diluted 10 5 times, take 100 μL of the diluted bacterial solution and evenly spread it on the solid culture medium (beef extract culture medium), place it in a constant temperature incubator at 37°C for 24 hours, and calculate the colony count (CFU / mL).
[0068] In this example, the number of E. coli in the blank control group and the three experimental groups changes with the sterilization time as shown in the following figure: Figure 4 As shown by Figure 4It can be seen that under neutral conditions, compared with the blank control group, the colony count of Escherichia coli did not change significantly when mFe was added for treatment, indicating that mFe basically has no ability to kill Escherichia coli. However, when mFe / nCu was added for treatment, the colony count of Escherichia coli decreased to a certain extent. When 0.5% C@mFe / nCu was added for treatment, the colony count of Escherichia coli decreased significantly, especially at 30 minutes of sterilization, 0.5% C@mFe / nCu was able to completely inhibit the growth and reproduction of Escherichia coli, indicating that 0.5% C@mFe / nCu has excellent bactericidal performance.
[0069] Example 4
[0070] In this embodiment, the micron-sized zero-valent iron (mFe for short) used in Example 1 and the micron-sized iron-copper bimetallic material (mFe / nCu for short) prepared in Comparative Example 1 were tested. Figure 5 In step (3) of Example 1, the carbon quantum dot-modified micron-sized zero-valent iron prepared when the amount of carbon quantum dots added in step (2) is 0.2 wt%, 0.5 wt%, and 0.8 wt% of the micron-sized zero-valent iron is used as the basis, and the amount of carbon quantum dot-modified micron-sized zero-valent iron added is controlled so that the mass ratio of copper to iron is 1:10, and the carbon quantum dot-modified micron-sized iron-copper bimetallic material (referred to as 0.2% C, 0.5% C, and 0.8% C, respectively) prepared is subjected to degradation performance of SMX.
[0071] (1) SMX was dissolved in deionized water and the pH value was adjusted to 3 to obtain SMX wastewater with an SMX concentration of 10 μmol / L.
[0072] (2) Take 5 portions of SMX wastewater, add mFe, 0% C, 0.2% C, 0.5% C, and 0.8% C to each portion of SMX wastewater, respectively, and control the concentration of mFe, 0% C, 0.2% C, 0.5% C, and 0.8% C in each portion of SMX wastewater to be 1 mg / mL. Stir and treat the wastewater at 30°C and 300 rpm for 30 minutes. During the wastewater treatment process, samples were taken every 5 to 10 minutes and filtered through a 0.22 μm filter membrane. The concentration of SMX was determined by HPLC, and the ratio of the final concentration C of SMX to its initial concentration C0 (C / C0) was calculated. A curve of the change of SMX C / C0 with reaction time was plotted.
[0073] Figure 5 The C / C0 curve of SMX changes with reaction time when mFe, 0% C, 0.2% C, 0.5% C, and 0.8% C are added in this embodiment (i.e., the degradation curve of SMX). Figure 5It can be seen that under the same dosage and water quality conditions, the degradation efficiency of SMX by 0.2% C, 0.5% C, and 0.8% C is higher than that by mFe and mFe / nCu, and the degradation efficiency of SMX by 0.5% C is the highest.
[0074] Example 5
[0075] In this embodiment, the degradation performance of SMX on the micron-sized zero-valent iron (abbreviated as mFe) used in Example 1 and the carbon quantum dot-modified micron-sized zero-valent iron prepared in step (3) of Example 1 when the amount of carbon quantum dots added in step (2) is 0.5 wt% of the micron-sized zero-valent iron is tested as the basis, and the amount of carbon quantum dot-modified micron-sized zero-valent iron added is controlled so that the mass ratio of copper to iron is 1:5, 1:10, 1:20, and 1:30, respectively, to prepare the carbon quantum dot-modified micron-sized iron-copper bimetallic material (abbreviated as Cu:Fe=1:5, Cu:Fe=1:10, Cu:Fe=1:20, and Cu:Fe=1:30).
[0076] (1) SMX was dissolved in deionized water and the pH value was adjusted to 3 to obtain SMX wastewater with an SMX concentration of 10 μmol / L.
[0077] (2) Take 5 portions of SMX wastewater and add mFe, Cu:Fe = 1:5, Cu:Fe = 1:10, Cu:Fe = 1:20, and Cu:Fe = 1:30 to each portion of SMX wastewater, respectively. Control the concentration of mZVI, Cu:Fe = 1:5, Cu:Fe = 1:10, Cu:Fe = 1:20, and Cu:Fe = 1:30 in each portion of SMX wastewater to be 1 mg / mL. Stir and treat the wastewater at 30°C and 300 rpm for 30 minutes. During the wastewater treatment process, samples were taken every 5 to 10 minutes and filtered through a 0.22 μm filter membrane. The concentration of SMX was determined by HPLC. The ratio of the final concentration C of SMX to its initial concentration C0, C / C0, was calculated, and a curve of the change of SMX C / C0 with reaction time was plotted.
[0078] Figure 6 The C / C0 curve of SMX changes with reaction time (i.e., the degradation curve of SMX) when mFe, Cu:Fe=1:5, Cu:Fe=1:10, Cu:Fe=1:20, and Cu:Fe=1:30 are added in this embodiment. Figure 6 It can be seen that under the same dosage and water quality conditions, the degradation efficiency of SMX by Cu:Fe=1:5, Cu:Fe=1:10, Cu:Fe=1:20, and Cu:Fe=1:30 is higher than that of mFe, and the degradation efficiency of SMX by Cu:Fe=1:5 and Cu:Fe=1:10 is significantly higher.
[0079] Example 6
[0080] In this embodiment, the degradation performance of the carbon quantum dot-modified micron-sized zero-valent iron (referred to as 0.5% C@mFe / nCu) prepared when the amount of carbon quantum dots added in step (2) of the micron-sized zero-valent iron is 0.5 wt% is tested in step (3) of Example 1 to test the degradation performance of the carbon quantum dot-modified micron-sized iron-copper bimetallic material (referred to as 0.5% C@mFe / nCu) on SMX wastewater with different pH values by controlling the amount of carbon quantum dot-modified micron-sized zero-valent iron added so that the mass ratio of copper to iron is 1:10.
[0081] (1) SMX was dissolved in deionized water to obtain an SMX solution with an SMX concentration of 10 μmol / L. Five portions of the SMX solution were taken and the pH values of each portion of the SMX solution were adjusted to 3, 4, 5, 6, and 7, respectively, to obtain SMX wastewater with different initial pH values.
[0082] (2) 0.5% C@mFe / nCu was added to SMX wastewater at different initial pH values. The concentration of 0.5% C@mFe / nCu in the SMX wastewater at different initial pH values was controlled to be 1 mg / mL. The wastewater was stirred at 30°C and 300 rpm for 30 min. During the wastewater treatment process, samples were taken every 5-10 min and filtered through a 0.22 μm filter membrane. The SMX concentration was determined by HPLC, and the SMX removal rate was calculated.
[0083] Figure 7 is the removal rate of SMX in SMX wastewater with different initial pH values by 0.5% C@mFe / nCu, Figure 7 It can be seen that when the pH value of the SMX wastewater is 3-6, the removal rate of SMX by 0.5% C@mFe / nCu can reach more than 70%. When the pH value of the SMX wastewater is 3-5, the removal rate of SMX by 0.5% C@mFe / nCu can reach 90%. When the pH value of the SMX wastewater is 3, SMX in the wastewater can be completely removed under the conditions of this embodiment. Compared with the traditional Fenton oxidation technology, the use of the carbon quantum dot-modified micron-sized iron-copper bimetallic material of the present invention can broaden the pH range of wastewater treatment to a certain extent, expanding the pH application range of the traditional Fenton oxidation technology from 2.8-3.5 to 3-5.
[0084] Example 7
[0085] In this embodiment, electron paramagnetic resonance (EPR) was used to test the types of active species generated when degrading pollutants by using the micron-sized zero-valent iron (mFe for short) used in Example 1, the micron-sized iron-copper bimetallic material (mFe / nCu for short) prepared in Comparative Example 1, and the carbon quantum dot-modified micron-sized zero-valent iron prepared in step (3) of Example 1 with the amount of carbon quantum dots added in step (2) being 0.5 wt % of the micron-sized zero-valent iron, and the carbon quantum dot-modified micron-sized iron-copper bimetallic material (0.5% C@mFe / nCu for short) prepared by controlling the amount of carbon quantum dots added to make the mass ratio of copper to iron be 1:10.
[0086] The types of capture agents added in the EPR test are: 5,5-dimethyl-1-pyrroline-N-oxide (DMPO) and 2,2,6,6-tetramethylpiperidinyl oxide (TEMP). DMPO can be used to capture hydroxyl radicals (·OH) and hydrogen radicals (*H) in water, and can be used to capture superoxide radicals (O2 ·- ), TEMP is used to capture singlet oxygen.
[0087] Adjust the pH value of deionized water to 3, take 3 portions of water with pH = 3, add mFe, mFe / Cu and 0.5% C@mFe / Cu to each portion of water with pH = 3, then add 10μL of capture agent DMPO, react for 1 to 4 minutes, take part of the mixture with a capillary, plug one end with plasticine, place the capillary into the resonance cavity, and perform electron paramagnetic resonance (EPR) test. The results are as follows Figure 8 As shown in Figure (a).
[0088] Take 3 portions of methanol, add mFe, mFe / Cu and 0.5% C@mFe / Cu to each portion of methanol, then add 10μL of free radical scavenger DMPO, react for 1 to 4 minutes, take part of the mixture with a capillary, plug one end with plasticine, place the capillary into the resonance cavity, and perform EPR measurement. The results are as follows Figure 8 As shown in Figure (b).
[0089] Adjust the pH value of deionized water to 3, take 3 portions of water with pH = 3, add mFe, mFe / Cu and 0.5% C@mFe / Cu to each portion of water with pH = 3, then add 10μL of capture agent TEMP, react for 1 to 4 minutes, take part of the mixture with a capillary, plug one end with plasticine, place the capillary into the resonance cavity, and perform EPR measurement. The results are as follows Figure 8 As shown in Figure (c).
[0090] Depend on Figure 8 It can be seen that the active species generated by the mFe system are ·OH and *H, and the active species generated by the mFe / Cu system are ·OH, *H and O2·- , the active species generated by the 0.5% C@mFe / Cu system are *H and O2 ·- .
[0091] Example 8
[0092] In this example, the effects of common anions and humic acid in water on the degradation of SMX by a carbon quantum dot-modified micron-sized iron-copper bimetallic material (referred to as 0.5% C@mFe / nCu) prepared by controlling the amount of carbon quantum dot-modified micron-sized zero-valent iron added so that the mass ratio of copper to iron is 1:10 in step (3) of Example 1, based on the carbon quantum dot-modified micron-sized zero-valent iron prepared when the amount of carbon quantum dots added in step (2) is 0.5 wt % of the micron-sized zero-valent iron, is investigated.
[0093] (1) Prepare SMX solution with deionized water and then add Cl - , the SMX concentration was 10 μmol / L, Cl - SMX solution with concentrations of 0, 1, 3, and 5 mmol / L was prepared and the pH value was adjusted to 3 to obtain simulated wastewater;
[0094] Prepare SMX solution with deionized water and add NO3 - , the SMX concentration was 10μmol / L, NO3 - SMX solution with concentrations of 0, 1, 3, and 5 mmol / L was prepared and the pH value was adjusted to 3 to obtain simulated wastewater;
[0095] An SMX solution was prepared with deionized water, and then humic acid (HA) was added to prepare SMX solutions with an SMX concentration of 10 μmol / L and HA concentrations of 0, 3, 5, and 10 mg / L, and the pH value was adjusted to 3 to obtain simulated wastewater.
[0096] (2) Take 300 mL of each simulated wastewater, place it in a 500 mL beaker, and place it in a constant temperature water bath at 30°C for 5 minutes. Then add 0.5% C@mFe / nCu to each simulated wastewater, control the concentration of 0.5% C@mFe / nCu in each simulated wastewater to be 1 mg / mL, and take 3 mL of samples at 5, 10, 20, 30, 60, 90, and 120 minutes after adding 0.5% C@mFe / nCu. Filter with a 0.22 μm filter membrane and put it into a sampling bottle. Determine the concentration of SMX by HPLC, calculate the ratio of the final concentration C of SMX to its initial concentration C0 C / C0, and draw a curve of the change of SMX C / C0 with reaction time. The results are shown in the figure. Figure 9 shown.
[0097] Depend on Figure 9It can be seen that low concentrations of anions Clˉ and NO3ˉ in water (for example, when the concentration does not exceed 5 mmol / L), and low concentrations of HA in water (for example, when the concentration does not exceed 10 mg / L), do not have a significant adverse effect on the ability of 0.5% C@mFe / nCu to degrade SMX, indicating that the carbon quantum dot-modified micron-sized iron-copper bimetallic material provided by the present invention can resist the adverse effects of low concentrations of common water matrices on its degradation of SMX.
[0098] Example 9
[0099] In this embodiment, the steps for preparing a carbon quantum dot modified micron-sized iron-copper bimetallic material are as follows:
[0100] (1) Synthesis of carbon quantum dots
[0101] Glucose was used as the carbon source. Glucose was added to deionized water and stirred thoroughly at room temperature until dissolved to obtain a glucose solution with a concentration of 5 g / L. Ammonia water was then added to adjust the pH value of the glucose solution to 6.5. Stirring was continued for 30 minutes to obtain a precursor solution. The precursor solution was transferred to a high-pressure reactor and reacted at 220°C for 5 hours. The resulting reaction solution was filtered through a 0.22 μm microporous membrane and dialyzed with a 500 MW dialysis bag for 2 days. The dialyzed reaction solution was freeze-dried to obtain carbon quantum dots.
[0102] (2) Preparation of micron-sized zero-valent iron modified with carbon quantum dots
[0103] Add micron-sized zero-valent iron with an average particle size of 40 μm and the carbon quantum dots prepared in step (1) into a ball mill, add zirconium oxide grinding balls into the ball mill, and ball mill at a speed of 300 rpm for 15 minutes to obtain micron-sized zero-valent iron modified with carbon quantum dots;
[0104] In this step, the mass ratio of the sum of the mass of the micron-sized zero-valent iron and the carbon quantum dots to the mass of the zirconia grinding balls is controlled to be 1:5, and the amount of the carbon quantum dots added is controlled to be 0.6 wt % of the micron-sized zero-valent iron.
[0105] (3) Copper loading on the surface of micron-sized zero-valent iron modified with carbon quantum dots
[0106] Copper sulfate pentahydrate is used as a copper source. The copper sulfate pentahydrate is added to deionized water and stirred at room temperature until dissolved to obtain a copper sulfate solution with a concentration of 2 mmol / L. The carbon quantum dot-modified micron-sized zero-valent iron prepared in step (2) is added, and the amount of the carbon quantum dot-modified micron-sized zero-valent iron added is controlled so that the mass ratio of copper to zero-valent iron is 1:5. The mixture is stirred at room temperature at a speed of 300 rpm for 5 minutes to perform a replacement reaction, and the solid-liquid separation is performed. The obtained solid phase is washed with deionized water to obtain a carbon quantum dot-modified micron-sized iron-copper bimetallic material.
[0107] The carbon quantum dots prepared in this example are used to modify the micron-sized iron-copper bimetallic material to degrade SMX wastewater:
[0108] SMX was dissolved in deionized water and the pH value was adjusted to 4 to obtain SMX wastewater with an SMX concentration of 15 μmol / L.
[0109] The carbon quantum dot-modified micron-sized iron-copper bimetallic material prepared in this example was added to the SMX wastewater at a concentration of 10 mg / mL. The wastewater was stirred at 30°C and 300 rpm for 30 minutes. After treatment, the wastewater was sampled and filtered through a 0.22 μm filter membrane. The SMX concentration was determined by HPLC, and the SMX removal rate was calculated. The results showed that the SMX removal rate was 99.3%.
[0110] Example 10
[0111] In this embodiment, the steps for preparing a carbon quantum dot modified micron-sized iron-copper bimetallic material are as follows:
[0112] (1) Synthesis of carbon quantum dots
[0113] Glutamic acid was used as a carbon source. The glutamate was added to deionized water and stirred thoroughly at room temperature until dissolved to obtain a glutamate solution with a concentration of 20 g / L. Ammonia water was then added to adjust the pH value of the glutamate solution to 6. Stirring was continued for 60 minutes to obtain a precursor solution. The precursor solution was transferred to a high-pressure reactor and reacted at 200°C for 6 hours. The resulting reaction solution was filtered through a 0.22 μm microporous membrane and dialyzed through a 500 MW dialysis bag for 3 days. The dialyzed reaction solution was freeze-dried to obtain carbon quantum dots.
[0114] (2) Preparation of micron-sized zero-valent iron modified with carbon quantum dots
[0115] Add micron-sized zero-valent iron with an average particle size of 120 μm and the carbon quantum dots prepared in step (1) into a ball mill, add zirconium oxide grinding balls into the ball mill, and ball mill for 60 minutes at a speed of 100 rpm to obtain micron-sized zero-valent iron modified with carbon quantum dots;
[0116] In this step, the mass ratio of the sum of the mass of the micron-sized zero-valent iron and the carbon quantum dots to the mass of the zirconia grinding balls is controlled to be 1:5, and the amount of the carbon quantum dots added is controlled to be 0.5 wt % of the micron-sized zero-valent iron.
[0117] (3) Copper loading on the surface of micron-sized zero-valent iron modified with carbon quantum dots
[0118] Copper sulfate pentahydrate was used as a copper source. Copper sulfate pentahydrate was added to deionized water and stirred at room temperature until dissolved to obtain a copper sulfate solution with a concentration of 20 mmol / L. The carbon quantum dot-modified micron-sized zero-valent iron prepared in step (2) was added. The amount of carbon quantum dot-modified micron-sized zero-valent iron added was controlled so that the mass ratio of copper to zero-valent iron was 1:6. The mixture was stirred at room temperature at a speed of 300 rpm for 4 minutes to carry out a replacement reaction. The solid-liquid separation was performed, and the obtained solid phase was washed with deionized water to obtain a carbon quantum dot-modified micron-sized iron-copper bimetallic material.
[0119] The carbon quantum dots prepared in this example are used to modify the micron-sized iron-copper bimetallic material to degrade SMX wastewater:
[0120] SMX was dissolved in deionized water and the pH value was adjusted to 3 to obtain SMX wastewater with an SMX concentration of 20 μmol / L.
[0121] The carbon quantum dot-modified micron-sized iron-copper bimetallic material prepared in this example was added to the SMX wastewater at a concentration of 100 mg / mL. The wastewater was stirred at 30°C and 300 rpm for 45 minutes. After the wastewater treatment was completed, a sample was filtered through a 0.22 μm filter membrane, and the SMX concentration was determined by HPLC. The SMX removal rate was calculated, and the results showed that the SMX removal rate was 100%.
Claims
1. A carbon quantum dot modified micron-sized iron-copper bimetallic material, characterized in that: The material consists of micron-sized zero-valent iron and carbon quantum dots and nano-copper particles loaded on the surface of the micron-sized zero-valent iron. The carbon quantum dots and nano-copper particles are evenly and discretely distributed on the surface of the micron-sized zero-valent iron.
2. According to claim 1, the carbon quantum dot modified micron-sized iron-copper bimetallic material is characterized in that: The particle size of the micron-sized zero-valent iron is 40 to 120 μm.
3. The method for preparing the carbon quantum dot modified micron-sized iron-copper bimetallic material according to claim 1 or 2, characterized in that: The following steps are involved: (1) adding micron-sized zero-valent iron and carbon quantum dots into a ball mill, controlling the amount of carbon quantum dots added to be 0.2 wt% to 0.8 wt% of the micron-sized zero-valent iron, adding grinding balls into the ball mill for thorough ball milling, and obtaining micron-sized zero-valent iron modified with carbon quantum dots; (2) adding the micron-sized zero-valent iron modified by carbon quantum dots to an aqueous solution of a divalent copper salt having a copper ion concentration of 2 to 20 mmol / L, controlling the amount of the micron-sized zero-valent iron modified by carbon quantum dots to be added so that the mass ratio of copper to zero-valent iron is 1:(5 to 10), performing a replacement reaction under stirring conditions, forming nano-copper particles on the surface of the micron-sized zero-valent iron modified by carbon quantum dots, performing solid-liquid separation, and washing the obtained solid phase with water to obtain a micron-sized iron-copper bimetallic material modified by carbon quantum dots.
4. The method for preparing the carbon quantum dot modified micron-sized iron-copper bimetallic material according to claim 3, characterized in that: The method for preparing carbon quantum dots comprises: dissolving a carbon source in water to form a carbon source solution with a concentration of 5 to 40 g / L, and adjusting the pH value of the carbon source solution to 6 to 6.5 to obtain a precursor solution; The precursor solution is transferred to a high-pressure reactor, reacted at 200-220° C. for 4-6 hours to obtain a reaction solution, the reaction solution is filtered through a microporous filter membrane and dialyzed with water for 2-3 days, and the dialyzed reaction solution is freeze-dried to obtain the product.
5. The method for preparing the carbon quantum dot modified micron-sized iron-copper bimetallic material according to claim 4, characterized in that: The carbon source is citric acid, glucose or glutamic acid.
6. The method for preparing the carbon quantum dot modified micron-sized iron-copper bimetallic material according to any one of claims 3 to 5, characterized in that: The time for carrying out the replacement reaction under stirring conditions in step (2) is 2 to 5 minutes.
7. Use of the carbon quantum dot-modified micron-sized iron-copper bimetallic material according to claim 1 or 2 in treating organic wastewater.
8. The use according to claim 6, characterized in that: The carbon quantum dot-modified micron-sized iron-copper bimetallic material according to claim 1 or 2 is added to wastewater containing organic pollutants, the pH value of the wastewater is controlled to be 3-5, the concentration of the carbon quantum dot-modified micron-sized iron-copper bimetallic material in the wastewater is controlled to be 1-100 mg / L, and the wastewater is treated under stirring conditions. The carbon quantum dot-modified micron-sized iron-copper bimetallic material generates superoxide radicals and hydrogen radicals during the wastewater treatment process to achieve the degradation of organic pollutants in the wastewater.
9. The use according to claim 8, characterized in that: When wastewater containing organic pollutants contains bacteria, the degradation of organic pollutants and the elimination of bacteria can be achieved simultaneously during the wastewater treatment process.
10. The use according to claim 8 or 9, characterized in that: The wastewater treatment time is determined according to the water quality of the organic wastewater.