Method for inhibiting initial activity of light olefin isomerization catalyst

By exchanging ammonium and calcining the silicon-aluminum molecular sieve, carbon deposit modification is achieved, and the problems of high initial activity and many side reactions of olefin isomerization catalysts are solved, and the selectivity and stability of the catalysts are improved. It is suitable for D- Isomerization reaction of ene and pentenyl backbone.

CN119016093APending Publication Date: 2024-11-26PETROCHINA CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202310593210.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing olefin isomerization catalyst has high initial activity, resulting in many side reactions such as olefin polymerization and cracking, resulting in loss of butene raw materials. The existing passivation treatment methods increase the process complexity, which is not conducive to industrial production.

Method used

By exchanging ammonium, drying and grinding on the silicon-aluminum molecular sieve, mixing with binder, extruding and calculating the organic template agent, carbon deposit modification is achieved, the initial activity of the catalyst is controlled, and the side reaction yield is reduced.

Benefits of technology

It effectively inhibits the initial reaction activity of the catalyst, reduces the side reaction of olefin polymerization and cracking, improves the selectivity and reactivity stability of isomer olefins, and extends the catalyst life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of olefin isomerization, in particular to a method for inhibiting initial activity of a light olefin isomerization catalyst, which comprises the following steps of: 1, performing ammonium exchange on a silicon-aluminum molecular sieve synthesized by an organic template agent to obtain an exchange molecular sieve, and drying and grinding the exchange molecular sieve to obtain exchange molecular sieve powder; 2, uniformly mixing the exchange molecular sieve powder with a required amount of a binder, adding sesbania powder and a dilute nitric acid solution, kneading, extruding and forming, and drying the extruded and formed catalyst to obtain a catalyst precursor; and 3, roasting the catalyst precursor, removing the organic template agent, and inhibiting the initial activity of the olefin skeletal isomerization catalyst subjected to carbon deposition modification. Inhibition of initial non-selective active sites of the catalyst can be achieved, isoolefin selectivity is effectively improved, meanwhile, the catalyst has excellent light olefin skeleton isomerization reaction activity stability, and the catalyst is long in service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of olefin isomerization, and is a method for inhibiting the initial activity of a light olefin isomerization catalyst, a carbon deposit-modified olefin skeletal isomerization catalyst and an application thereof. Background Art

[0002] The C4 fraction cracked by the refinery contains rich butene components. After the mixed C4 reacts with methanol to generate MTBE (methyl tert-butyl ether), there are still a large number of normal butenes. These butenes can further generate isobutylene through skeletal isomerization reaction to achieve the purpose of increasing MTBE production. In addition, high-purity isobutylene can be produced by cracking MTBE, which can be widely used in the production of various chemical products such as butyl rubber, polyisobutylene, methyl methacrylate (MMA), tert-butyl alcohol, tert-butyl phenol, antioxidants, tert-butylamine, etc. Therefore, the technology of producing isobutylene by skeletal isomerization reaction of butene has attracted widespread attention.

[0003] Catalysts for the skeletal isomerization of light straight-chain olefins can be mainly divided into three categories: halide catalysts, non-halide catalysts and molecular sieve catalysts. At present, the research focus is mainly on molecular sieve catalysts, especially ferrous alkali zeolite molecular sieves with FER structure. When FER molecular sieve is used as a catalyst for the skeletal isomerization of butene, due to the presence of non-selective active centers on the surface of the molecular sieve, in the process of skeletal isomerization of n-butene, in addition to the skeletal isomerization of olefins to form isobutylene, side reactions such as olefin dimerization and cracking occur, generating propylene and liquid products with C5 or higher oligomers. This phenomenon is more prominent in the initial stage of the reaction when the catalyst has the strongest non-selective activity, the reaction releases a large amount of heat, and a large amount of propylene and liquid oligomers are generated, resulting in a large loss of butene raw materials. Therefore, it is necessary to develop a method for inhibiting the initial activity of olefin isomerization catalysts to achieve the purpose of inhibiting the initial reaction activity of the catalyst and reducing the occurrence of side reactions such as olefin polymerization and cracking.

[0004] The Chinese patent document with publication number CN103785482A discloses a passivation treatment method for an olefin isomerization catalyst, which specifically comprises the following steps: (1) introducing a heavy by-product of an olefin isomerization process as a passivating agent, either alone or together with an olefin isomerization reaction raw material, into a catalyst bed prepared with HZSM-35 molecular sieve as a main active component to contact the olefin isomerization catalyst for 3 to 7 hours, thereby passivating the molecular sieve catalyst; (2) then, under conditions of a pressure of 0.01 to 0.2 MPa and a reaction temperature of 310 to 450°C, the catalyst is passivated for 0.5 to 2.0 h. -1After the ether is introduced at a mass space velocity of , the carbon tetrachloride is used to carry out the butene skeletal isomerization reaction; (3) After the catalyst is passivated by this method, the selectivity of the catalyst for the butene skeletal isomerization reaction is significantly improved, and the polymerization by-products are significantly reduced. Within 3 hours of the initial reaction, the isobutylene selectivity is increased from 52.81% to 77.25%, and the heavy oil yield is reduced from 18.71% to 8.96%. The method of the invention can suppress the initial activity of the light olefin isomerization catalyst, but the method requires the additional addition of the passivating agent feed at the initial stage of the olefin isomerization catalyst reaction, which increases the complexity of the isomerization reaction process operation and is not conducive to the promotion and application in large-scale industrial production. Summary of the invention

[0005] The present invention provides a method for inhibiting the initial activity of a light olefin isomerization catalyst, which overcomes the deficiencies of the above-mentioned prior art and can effectively solve the problems of high initial reaction activity of the prior art catalyst and many side reactions such as olefin polymerization and cracking.

[0006] One of the technical solutions of the present invention is achieved by the following measures: A method for inhibiting the initial activity of a light olefin isomerization catalyst is carried out according to the following steps: The first step is to perform ammonium exchange on the silicon-aluminum molecular sieve synthesized by the organic template to obtain an exchange molecular sieve, and then dry and grind the exchange molecular sieve to obtain an exchange molecular sieve powder; The second step is to evenly mix the exchange molecular sieve powder with a required amount of a binder, add sesbania powder and a dilute nitric acid solution, knead and extrude into strips, and dry the extruded catalyst to obtain a catalyst precursor; The third step is to calcine the catalyst precursor to remove the organic template, and the initial activity of the olefin skeletal isomerization catalyst after carbon deposition modification is suppressed.

[0007] The following are further optimizations and / or improvements to the above technical solutions: In the first step, the silica-alumina molecular sieve includes but is not limited to ZSM-5, ZSM-35, and ZSM-22 molecular sieves; or / and, the organic template agent includes but is not limited to pyridine, ethylenediamine, cyclohexylamine, and n-butene.

[0008] In the first step, the silicon-alumina molecular sieve is ZSM-35 molecular sieve; or / and the organic template is cyclohexylamine.

[0009] In the first step, the silica-alumina molecular sieve is exchanged with ammonium salt, wherein the ammonium salt is an aqueous solution of ammonium chloride, and the conditions for the ammonium exchange are: the concentration of the aqueous solution of ammonium chloride is 1 mol / L, the exchange temperature is 80°C, the liquid-solid ratio of the aqueous solution of ammonium chloride to the silica-alumina molecular sieve is 10:1, and the number of exchanges is 2 to 4 times.

[0010] In the above second step, the binder includes but is not limited to pseudo-boehmite, aluminum hydroxide, silica sol, and / or, and the mass ratio of the exchange molecular sieve powder to the binder is 9:1 to 5:5.

[0011] In the second step, the binder is pseudo-boehmite; or / and the mass ratio of the exchange molecular sieve powder to the binder is 8:2.

[0012] In the above-mentioned second step, the drying temperature is 100°C to 150°C, and the drying time is 2 hours to 12 hours; or / and, in the third step, the roasting conditions are: the roasting temperature is 350°C to 550°C, the roasting atmosphere is a nitrogen-air mixture or air, the volume content of oxygen in the nitrogen-air mixture is 0 to 21%, and the roasting time is 2 hours to 12 hours.

[0013] The second technical solution of the present invention is achieved by the following measures: a carbon deposit-modified olefin skeletal isomerization catalyst is prepared according to the following steps: The first step is to perform ammonium exchange on the silicon-aluminum molecular sieve synthesized by the organic template to obtain an exchange molecular sieve, and then dry and grind the exchange molecular sieve to obtain an exchange molecular sieve powder; The second step is to evenly mix the exchange molecular sieve powder with a required amount of a binder, add sesbania powder and a dilute nitric acid solution, knead and extrude into strips, and dry the extruded catalyst to obtain a catalyst precursor; The third step is to calcine the catalyst precursor to remove the organic template, thereby obtaining a carbon deposit-modified olefin skeletal isomerization catalyst.

[0014] The third technical solution of the present invention is achieved by the following measures: application of a carbon deposit-modified olefin skeletal isomerization catalyst to a light olefin skeletal isomerization reaction, wherein the light olefin skeletal isomerization reaction includes a butene skeletal isomerization reaction and a pentene skeletal isomerization reaction.

[0015] The above-mentioned butene skeletal isomerization reaction uses etherified C4 as raw material and adopts a carbon deposition modified olefin skeletal isomerization catalyst for catalytic reaction. The reaction conditions are: reaction temperature of 300°C to 450°C, reaction pressure of 0.1MPa to 0.2MPa, raw material feed mass space velocity of 2.0h -1 To 10.0h -1 The pentene skeletal isomerization reaction uses etherified carbon five as raw material and adopts a carbon deposition modified olefin skeletal isomerization catalyst for catalytic reaction. The reaction conditions are: reaction temperature is 250℃ to 400℃, reaction pressure is 0.2MPa to 0.5MPa, and raw material feed mass space velocity is 2.0h -1 To 10.0h -1 .

[0016] The present invention achieves the purpose of pre-carbon modification of the catalyst by controlling the removal conditions of the organic template agent, thereby suppressing the initial non-selective active sites of the catalyst, reducing the yield of olefin polymerization liquid products in the initial reaction of the catalyst, and effectively improving the isoolefin selectivity. At the same time, it has excellent light olefin skeletal isomerization reaction activity stability and a long catalyst life. DETAILED DESCRIPTION

[0017] The present invention is not limited by the following embodiments, and the specific implementation method can be determined according to the technical scheme of the present invention and the actual situation. Unless otherwise specified, the various chemical reagents and chemicals mentioned in the present invention are all known and commonly used chemical reagents and chemicals in the prior art; the percentages in the present invention are all mass percentages unless otherwise specified; the solutions in the present invention are all aqueous solutions with water as the solvent unless otherwise specified, for example, a dilute nitric acid solution is a dilute nitric acid aqueous solution; the normal temperature and room temperature in the present invention generally refer to a temperature of 15°C to 25°C, and are generally defined as 25°C.

[0018] The present invention will be further described below in conjunction with embodiments: Example 1: The method for suppressing the initial activity of a light olefin isomerization catalyst is carried out according to the following steps: The first step is to perform ammonium exchange on the silicon-aluminum molecular sieve synthesized by the organic template to obtain an exchange molecular sieve, and then dry and grind the exchange molecular sieve to obtain an exchange molecular sieve powder; The second step is to evenly mix the exchange molecular sieve powder with a required amount of a binder, add sesbania powder and a dilute nitric acid solution, knead and extrude into strips, and dry the extruded catalyst to obtain a catalyst precursor; The third step is to calcine the catalyst precursor to remove the organic template, and the initial activity of the olefin skeletal isomerization catalyst after carbon deposition modification is suppressed.

[0019] The invention provides a method for inhibiting the initial activity of a light olefin isomerization catalyst. The method comprises the following steps: performing ammonium exchange on a silicon-aluminum molecular sieve synthesized by an organic template agent, kneading the resulting mixture with a binder, extruding the mixture into strips, and drying the mixture to obtain a catalyst precursor. The catalyst precursor is then calcined under certain conditions to remove a portion of the template agent, thereby obtaining a carbon-deposition-modified olefin isomerization catalyst. The method inhibits the initial activity of the catalyst reaction, reduces side reactions such as olefin polymerization and cracking, and improves the selectivity of isomerized olefins. The olefin skeletal isomerization catalyst prepared by the method has low polymerization liquid yield and good isomerized olefin selectivity at the initial stage of the reaction, and also has excellent light olefin skeletal isomerization reaction activity stability and a long catalyst life.

[0020] Example 2: As an optimization of the above example, in the first step, the silica-alumina molecular sieve includes but is not limited to ZSM-5, ZSM-35, ZSM-22 molecular sieves; or / and, the organic template agent includes but is not limited to pyridine, ethylenediamine, cyclohexylamine, and n-butene.

[0021] Example 3: As an optimization of the above example, in the first step, the silica-alumina molecular sieve is a ZSM-35 molecular sieve; or / and, the organic template is cyclohexylamine.

[0022] Example 4: As an optimization of the above example, in the first step, the ammonium salt is used to exchange the silica-alumina molecular sieve with ammonium, wherein the ammonium salt is an ammonium chloride aqueous solution, and the ammonium exchange conditions are: the concentration of the ammonium chloride aqueous solution is 1 mol / L, the exchange temperature is 80°C, the liquid-solid ratio of the ammonium chloride aqueous solution to the silica-alumina molecular sieve is 10:1, and the number of exchanges is 2 to 4 times.

[0023] Example 5: As an optimization of the above example, in the second step, the binder includes but is not limited to pseudo-boehmite, aluminum hydroxide, silica sol, or / and, and the mass ratio of the exchange molecular sieve powder to the binder is 9:1 to 5:5.

[0024] Example 6: As an optimization of the above example, in the second step, the binder is pseudo-boehmite; or / and, the mass ratio of the exchange molecular sieve powder to the binder is 8:2.

[0025] Embodiment 7: As an optimization of the above embodiment, in the second step, the drying temperature is 100°C to 150°C, and the drying time is 2 hours to 12 hours; or / and, in the third step, the roasting conditions are: the roasting temperature is 350°C to 550°C, the roasting atmosphere is a nitrogen-air mixture or air, the volume content of oxygen in the nitrogen-air mixture is 0 to 21%, and the roasting time is 2 hours to 12 hours. The roasting process is carried out in a programmed temperature mode.

[0026] Example 8: The carbon deposit-modified olefin skeletal isomerization catalyst is prepared according to the following steps: The first step is to perform ammonium exchange on the silicon-aluminum molecular sieve synthesized by the organic template to obtain an exchange molecular sieve, and then dry and grind the exchange molecular sieve to obtain an exchange molecular sieve powder; The second step is to evenly mix the exchange molecular sieve powder with a required amount of a binder, add sesbania powder and a dilute nitric acid solution, knead and extrude into strips, and dry the extruded catalyst to obtain a catalyst precursor; The third step is to calcine the catalyst precursor to remove the organic template, thereby obtaining a carbon deposit-modified olefin skeletal isomerization catalyst.

[0027] Example 9: Application of a carbon deposit-modified olefin skeletal isomerization catalyst in a light olefin skeletal isomerization reaction, wherein the light olefin skeletal isomerization reaction includes a butene skeletal isomerization reaction and a pentene skeletal isomerization reaction.

[0028] Example 10: As an optimization of the above example, the butene skeletal isomerization reaction uses etherified C4 as raw material and adopts a carbon deposition modified olefin skeletal isomerization catalyst for catalytic reaction. The reaction conditions are: reaction temperature of 300°C to 450°C, reaction pressure of 0.1MPa to 0.2MPa, and raw material feed mass space velocity of 2.0h -1 To 10.0h -1 In the initial 3 hours of the butene skeletal isomerization reaction, the liquid product yield is 2% to 6%, the isobutylene selectivity is 70% to 90%, and the isobutylene yield is 30% to 40%; the catalyst can operate continuously for 600 to 1200 hours in a single pass, with an isobutylene selectivity of 85% to 98% and an isobutylene yield of 30% to 40%.

[0029] Example 11: As an optimization of the above example, the pentene skeletal isomerization reaction uses etherified carbon five as raw material, and adopts a carbon deposition modified olefin skeletal isomerization catalyst for catalytic reaction. The reaction conditions are: reaction temperature is 250°C to 400°C, reaction pressure is 0.2MPa to 0.5MPa, and raw material feed mass space velocity is 2.0h -1 To 10.0h -1 . 1-pentene, cis-2-pentene and trans-2-pentene in the pentene skeletal isomerization reaction raw materials are collectively referred to as n-pentene, and the reaction products 2-methyl-1-butene and 2-methyl-2-butene are collectively referred to as active olefins. Within the initial 3 hours of the reaction, the yield of the polymerized liquid product is 1% to 3%, the selectivity of active olefins is 70% to 90%, and the yield of active olefins is 50% to 70%; the catalyst can run continuously for 600 to 1200 hours in a single pass, the selectivity of active olefins is 90% to 98%, and the yield of active olefins is 50% to 70%.

[0030] Example 12: Take 100 grams of ZSM-35 molecular sieve powder synthesized using cyclohexylamine as a template, exchange with ammonium chloride solution (concentration 1 mol / L) 10 times the mass of the molecular sieve powder at 80°C for 2 hours, wash the filter cake with deionized water until no chloride ions remain, and repeat the exchange once, and dry the filter cake at 100°C for 4 hours after washing. After grinding, the dried molecular sieve is evenly mixed with alumina at a mass ratio of 8:2, and 2 grams of sesbania powder and 3% mass concentration of dilute nitric acid are added to knead and extrude into strips, and the extruded catalyst is dried at 120°C for 6 hours to obtain a catalyst precursor. The dried catalyst precursor was crushed into 1mm to 2mm particles and placed in a muffle furnace for calcination. The temperature program was: 25°C was heated to 300°C for 2 hours and then calcined for 2 hours, then 300°C was heated to 440°C for 2 hours and then calcined for 2 hours. After calcination, the catalyst was taken out after cooling down to obtain a carbon deposition modified olefin skeletal isomerization catalyst. The sample was recorded as S1. The carbon deposition analysis of sample S1 was performed, and the carbon deposition amount of sample S1 was calculated to be 4.6%.

[0031] Example 13: Take 100 grams of ZSM-35 molecular sieve powder synthesized using cyclohexylamine as a template, exchange with ammonium chloride solution (concentration 1 mol / L) 10 times the mass of the molecular sieve powder at 80°C for 2 hours, wash the filter cake with deionized water until no chloride ions remain, and repeat the exchange once, and dry the filter cake at 100°C for 4 hours after washing. After grinding, the dried molecular sieve is evenly mixed with alumina at a mass ratio of 8:2, and 2 grams of sesbania powder and 3% dilute nitric acid are added to knead and extrude into strips. The extruded catalyst is dried at 120°C for 6 hours to obtain a catalyst precursor. The dried catalyst precursor was crushed into 1mm to 2mm particles and placed in a muffle furnace for calcination. The heating program was: 25°C was heated to 300°C for 2 hours and then calcined for 2 hours, then 300°C was heated to 460°C for 2 hours and then calcined for 2 hours. After calcination, the catalyst was taken out after cooling down to obtain a carbon deposition modified olefin skeletal isomerization catalyst, and the sample was recorded as S2. The carbon deposition analysis of sample S2 was performed, and the carbon deposition amount of sample S2 was calculated to be 3.5%.

[0032] Example 14: Take 100 grams of ZSM-35 molecular sieve powder synthesized using cyclohexylamine as a template, exchange with ammonium chloride solution (concentration 1 mol / L) 10 times the mass of the molecular sieve powder at 80°C for 2 hours, wash the filter cake with deionized water until no chloride ions remain, and repeat the exchange once, and dry the filter cake at 100°C for 4 hours after washing. After grinding, the dried molecular sieve is evenly mixed with alumina at a mass ratio of 8:2, and 2 grams of sesbania powder and 3% dilute nitric acid are added to knead and extrude into strips. After extrusion, the catalyst is dried at 120°C for 6 hours to obtain a catalyst precursor. The dried catalyst precursor was crushed into 1mm to 2mm particles and placed in a muffle furnace for calcination. The temperature program was: 25°C was heated to 300°C for 2 hours and then calcined at a constant temperature for 2 hours. 300°C was heated to 480°C for 3 hours and then calcined at a constant temperature for 2 hours. After calcination, the catalyst was taken out after cooling down to obtain a carbon deposition modified olefin skeletal isomerization catalyst, and the sample was recorded as S3. The carbon deposition analysis of sample S3 was performed, and the carbon deposition amount of sample S3 was calculated to be 2.6%.

[0033] Example 15: Take 100 grams of ZSM-35 molecular sieve powder synthesized using cyclohexylamine as a template, exchange with ammonium chloride solution (concentration 1 mol / L) 10 times the mass of the molecular sieve powder at 80°C for 2 hours, wash the filter cake with deionized water until no chloride ions remain, and repeat the exchange once, and dry the filter cake at 100°C for 4 hours after washing. After grinding, the dried molecular sieve is evenly mixed with alumina at a mass ratio of 8:2, and 2 grams of sesbania powder and 3% dilute nitric acid are added to knead and extrude into strips. After extrusion, the catalyst is dried at 120°C for 6 hours to obtain a catalyst precursor. The dried catalyst precursor was crushed into particles of 1 mm to 2 mm, 30 g of the catalyst precursor was loaded into a fixed bed reactor, and calcined in an atmosphere with a nitrogen flow rate of 20 liters per hour and an air flow rate of 20 liters per hour, and the temperature program was as follows: 25°C was heated to 300°C for 2 hours and then calcined at a constant temperature for 2 hours, and then 300°C was heated to 440°C for 2 hours and then calcined at a constant temperature for 2 hours. After calcination, the catalyst was taken out after cooling down, and a carbon deposition-modified olefin skeletal isomerization catalyst was obtained, and the sample was recorded as S4. The carbon deposition analysis of sample S4 was performed, and the carbon deposition amount of sample S4 was calculated to be 4.5%.

[0034] Example 16: Take 100 grams of ZSM-35 molecular sieve powder synthesized using cyclohexylamine as a template, exchange with ammonium chloride solution (concentration 1 mol / L) 10 times the mass of the molecular sieve powder at 80°C for 2 hours, wash the filter cake with deionized water until no chloride ions remain, and repeat the exchange once, and dry the filter cake at 100°C for 4 hours after washing. After grinding, the dried molecular sieve is evenly mixed with alumina at a mass ratio of 8:2, and 2 grams of sesbania powder and 3% mass concentration of dilute nitric acid are added to knead and extrude into strips. After extrusion, the catalyst is dried at 120°C for 6 hours to obtain a catalyst precursor. The dried catalyst precursor was crushed into particles of 1 mm to 2 mm, 30 g of the catalyst precursor was loaded into a fixed bed reactor, and calcined in an atmosphere of 20 liters per hour of nitrogen and 20 liters per hour of air, and the temperature program was as follows: 25°C was heated to 300°C for 2 hours and then calcined at a constant temperature for 2 hours, and then 300°C was heated to 460°C for 2 hours and then calcined at a constant temperature for 2 hours. After calcination, the catalyst was taken out after cooling down, and a carbon deposition-modified olefin skeletal isomerization catalyst was obtained, and the sample was recorded as S5. The carbon deposition analysis of sample S5 was performed, and the carbon deposition amount of sample S5 was calculated to be 3.4%.

[0035] Example 17: Take 100 grams of ZSM-35 molecular sieve powder synthesized using cyclohexylamine as a template, exchange with ammonium chloride solution (concentration 1 mol / L) 10 times the mass of the molecular sieve powder at 80°C for 2 hours, wash the filter cake with deionized water until no chloride ions remain, and repeat the exchange once, and dry the filter cake at 100°C for 4 hours after washing. After grinding, the dried molecular sieve is evenly mixed with alumina at a mass ratio of 8:2, and 2 grams of sesbania powder and 3% mass concentration of dilute nitric acid are added to knead and extrude into strips. After extrusion, the catalyst is dried at 120°C for 6 hours to obtain a catalyst precursor. The dried catalyst precursor was crushed into 1mm to 2mm particles, 30g of the catalyst precursor was loaded into a fixed bed reactor, and calcined in an atmosphere with a nitrogen flow rate of 20 liters per hour and an air flow rate of 20 liters per hour. The temperature program was: 25°C was heated to 300°C for 2 hours and then calcined at a constant temperature for 2 hours, and then 300°C was heated to 480°C for 3 hours and then calcined at a constant temperature for 2 hours. After calcination, the catalyst was taken out after cooling down to obtain a carbon deposition modified olefin skeletal isomerization catalyst, and the sample was recorded as S6. The carbon deposition analysis of sample S6 was performed, and the carbon deposition amount of sample S6 was calculated to be 2.5%.

[0036] The amount of carbon deposits in the carbon deposit modified olefin skeletal isomerization catalysts obtained in Examples 12 to 17 was analyzed and calculated using a Mettler-Toledo TGA / DSC-1 / 1600 thermal analyzer. The results of the carbon deposit modified olefin skeletal isomerization catalysts prepared in Examples 12 to 17 are shown in Table 1.

[0037] The carbon deposit modified olefin skeletal isomerization catalyst prepared in Examples 12 to 17 was used, and the etherified C4 of the refinery was used as the raw material to carry out the butene skeletal isomerization reaction. The reaction activity, selectivity and life of the carbon deposit modified olefin skeletal isomerization catalyst prepared in Examples 12 to 17 were evaluated using a fixed bed evaluation device with a catalyst loading of 100 mL. The reaction temperature was 350° C., the reaction pressure was 0.1 MPa, and the mass space velocity of the etherified C4 was 5.5 h -1 .

[0038] The reaction product was analyzed for all components by online chromatography. The isobutylene selectivity, liquid product yield, and isobutylene yield were calculated according to the following formulas (1) to (3): .

[0039] The evaluation results of the initial 3 hours of the reaction are shown in Table 2, and the results of the catalyst long-term operation reaction are shown in Table 3. It can be concluded from Tables 2 and 3 that when the olefin skeletal isomerization catalyst prepared by the method provided by the present invention is used for the butene skeletal isomerization reaction, the liquid product yield is between 2.1% and 5.6% within the initial 3 hours of the reaction, the isobutylene selectivity is between 76.2% and 87.3%, and the isobutylene yield is between 32.9% and 35.7%; the catalyst can be continuously operated for more than 800 hours in a single pass, with an isobutylene selectivity of 92.1% to 95.3% and an isobutylene yield of 33.8% to 38.1%. It shows that the method of the present invention achieves the suppression of the initial non-selective active sites of the catalyst, reduces the yield of the olefin polymerization liquid product of the initial reaction of the catalyst, and effectively improves the selectivity of isomerized olefins.

[0040] The carbon deposit-modified olefin skeletal isomerization catalyst prepared in Examples 12 to 17 was used to carry out pentene skeletal isomerization reaction with the etherified C5 of the refinery as raw material. The reaction activity, selectivity and life of the carbon deposit-modified olefin skeletal isomerization catalyst prepared in Examples 12 to 17 were evaluated using a fixed bed evaluation device with a catalyst loading of 100 mL. The reaction temperature was 300°C, the reaction pressure was 0.3 MPa, the mass space velocity of the etherified C5 was 3.0 h-1, and the evaluation results for the initial 3 hours of the reaction are shown in Table 4. The reaction results of the long-term operation of the catalyst are shown in Table 5. It can be concluded from Table 4 and Table 5 that when the olefin skeleton isomerization catalyst prepared by the method provided by the present invention is used for the pentene skeleton isomerization reaction, the yield of the polymerized liquid product is between 1.2% and 3.1% within the initial 3 hours of the reaction, the active olefin selectivity is between 82.5% and 92.1%, and the active olefin yield is between 51.1% and 58.7%; the catalyst can be continuously operated for more than 1000 hours in a single pass, with an active olefin selectivity of 95.2% to 97.1%, and an active olefin yield of 57.8% to 65.1%. This indicates that the method of the present invention achieves the suppression of the initial non-selective active sites of the catalyst, reduces the yield of the olefin polymerization liquid product of the initial reaction of the catalyst, and effectively improves the isoolefin selectivity.

[0041] In summary, the present invention provides a method for inhibiting the initial activity of an olefin skeletal isomerization catalyst. The method achieves the purpose of pre-carbon modification of the catalyst by controlling the removal conditions of the organic template, thereby inhibiting the initial non-selective active sites of the catalyst, reducing the yield of olefin polymerization liquid products in the initial reaction of the catalyst, and effectively improving the selectivity of isomerized olefins. At the same time, the method has excellent light olefin skeletal isomerization reaction activity stability and a long catalyst life.

[0042] The above technical features constitute the embodiments of the present invention, which have strong adaptability and implementation effect. Non-essential technical features can be added or reduced according to actual needs to meet the requirements of different situations.

Claims

1. A method for inhibiting the initial activity of a light olefin isomerization catalyst, Features Follow these steps: The first step is to perform ammonium exchange on the silicon-aluminum molecular sieve synthesized by the organic template to obtain an exchange molecular sieve, and then dry and grind the exchange molecular sieve to obtain an exchange molecular sieve powder; The second step is to evenly mix the exchange molecular sieve powder with a required amount of a binder, add sesbania powder and a dilute nitric acid solution, knead and extrude into strips, and dry the extruded catalyst to obtain a catalyst precursor; The third step is to calcine the catalyst precursor to remove the organic template, and the initial activity of the olefin skeletal isomerization catalyst after carbon deposition modification is suppressed.

2. The method for suppressing the initial activity of a light olefin isomerization catalyst according to claim 1, Features In the first step, the silica-alumina molecular sieve includes but is not limited to ZSM-5, ZSM-35, and ZSM-22 molecular sieves; or / and, the organic template agent includes but is not limited to pyridine, ethylenediamine, cyclohexylamine, and n-butene.

3. The method for suppressing the initial activity of a light olefin isomerization catalyst according to claim 2, Features In the first step, the silica-alumina molecular sieve is ZSM-35 molecular sieve; or / and, the organic template is cyclohexylamine.

4. The method for suppressing the initial activity of a light olefin isomerization catalyst according to any one of claims 1 to 3, Features In the first step, the silica-alumina molecular sieve is exchanged with ammonium salt, wherein the ammonium salt is an aqueous solution of ammonium chloride, and the conditions for the ammonium exchange are: the concentration of the aqueous solution of ammonium chloride is 1 mol / L, the exchange temperature is 80°C, the liquid-solid ratio of the aqueous solution of ammonium chloride to the silica-alumina molecular sieve is 10:1, and the number of exchanges is 2 to 4 times.

5. The method for suppressing the initial activity of a light olefin isomerization catalyst according to any one of claims 1 to 4, Features In the second step, the binder includes but is not limited to pseudo-boehmite, aluminum hydroxide, silica sol, and / or the mass ratio of the exchange molecular sieve powder to the binder is 9:1 to 5:

5.

6. The method for suppressing the initial activity of a light olefin isomerization catalyst according to any one of claims 1 to 5, Features In the second step, the binder is pseudo-boehmite; or / and the mass ratio of the exchange molecular sieve powder to the binder is 8:

2.

7. The method for suppressing the initial activity of a light olefin isomerization catalyst according to claims 1 to 6, Features In the second step, the drying temperature is 100°C to 150°C, and the drying time is 2 hours to 12 hours; or / and, in the third step, the roasting conditions are: the roasting temperature is 350°C to 550°C, the roasting atmosphere is a nitrogen-air mixture or air, the volume content of oxygen in the nitrogen-air mixture is 0 to 21%, and the roasting time is 2 hours to 12 hours.

8. A carbon deposit-modified olefin skeletal isomerization catalyst prepared by the method for suppressing the initial activity of a light olefin isomerization catalyst according to claims 2 to 7, Features Prepared according to the following steps: The first step is to perform ammonium exchange on the silicon-aluminum molecular sieve synthesized by the organic template to obtain an exchange molecular sieve, and then dry and grind the exchange molecular sieve to obtain an exchange molecular sieve powder; The second step is to evenly mix the exchange molecular sieve powder with a required amount of a binder, add sesbania powder and a dilute nitric acid solution, knead and extrude into strips, and dry the extruded catalyst to obtain a catalyst precursor; The third step is to calcine the catalyst precursor to remove the organic template, thereby obtaining a carbon deposit-modified olefin skeletal isomerization catalyst.

9. Use of the carbon deposit-modified olefin skeletal isomerization catalyst according to claim 8 in a light olefin skeletal isomerization reaction, Features The light olefin skeletal isomerization reaction includes butene skeletal isomerization reaction and pentene skeletal isomerization reaction.

10. Use of the carbon deposit-modified olefin skeletal isomerization catalyst according to claim 9 in a light olefin skeletal isomerization reaction, Features The butene skeletal isomerization reaction uses etherified C4 as raw material and adopts a carbon deposition modified olefin skeletal isomerization catalyst for catalytic reaction. The reaction conditions are: reaction temperature is 300℃ to 450℃, reaction pressure is 0.1MPa to 0.2MPa, and raw material feed mass space velocity is 2.0h -1 To 10.0h -1 The pentene skeletal isomerization reaction uses etherified carbon five as raw material and adopts a carbon deposition modified olefin skeletal isomerization catalyst for catalytic reaction. The reaction conditions are: reaction temperature is 250℃ to 400℃, reaction pressure is 0.2MPa to 0.5MPa, and raw material feed mass space velocity is 2.0h -1 To 10.0h -1 .

Citation Information

Patent Citations

  • Method for improving butene double bond isomerization reaction

    CN101475432A

  • Catalyst for preparing isobutene by n-butene isomerization as well as preparation method and application of catalyst

    CN104549451A

  • Method for isomerizing butene-2 into butene-1

    CN105272800A

  • Molecular sieve catalyst, and preparation method and application thereof

    CN106824257A

  • Preparation method for straight-chain olefin framework isomerization catalyst

    CN108114735A