Catalyst for producing biodiesel and preparation method thereof
By using supercritical fluid to prepare inorganic acid/MOF-808 catalyst in the production of biodiesel catalysts, the problems of low catalyst conversion and poor reuse performance are solved, and more efficient biodiesel synthesis and long-term stability of catalysts are achieved. sex.
Patent Information
- Application Number
- CN202411113696.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
The conversion rate of existing biodiesel catalysts is low and the catalyst reuse performance is poor. In particular, the active components of the inorganic acid/MOF catalysts are unevenly dispersed and easily lost in the traditional impregnation method, which affects the catalytic effect.
The method of preparing inorganic acid/MOF-808 catalysts using supercritical fluids is used to dissolve 1,3,5-benzenetriacetic acid and zirconium salts in N,N-dimethylformamide and formic acid, followed by supercritical The temperature-raising and pressurization treatment in the fluid ensures uniform dispersion of the inorganic acid on the MOF-808 material and strong support action.
The dispersion uniformity and reusability of the active components of the catalyst are improved, the conversion rate of oleic acid and methanol is significantly improved, the loss rate of active components is reduced, and the service life of the catalyst is extended.
Smart Images

Figure BDA0004993036690000071 
Figure BDA0004993036690000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biodiesel catalysts, and in particular to a catalyst used for producing biodiesel and a preparation method thereof. Background Art
[0002] Biodiesel is widely recognized as a new energy source that can replace petrochemical diesel. It has the advantages of being renewable, environmentally friendly, biodegradable and safe. Compared with traditional petrochemical diesel, biodiesel made from waste oils from the catering and food industries can reduce greenhouse gas emissions by about 80%. Chemical esterification using solid acid as a catalyst is currently the main method for preparing biodiesel. However, the esterification reaction still has problems such as low conversion rate and poor catalyst reusability.
[0003] Metal-organic framework materials (MOFs) are an emerging catalyst with many unique advantages, such as porosity, high specific surface area, structural diversity, and functional adjustability. Inorganic acid-modified MOFs materials are a type of catalyst with excellent catalytic performance, which can achieve a good conversion rate in the synthesis of biodiesel from oleic acid and methanol esterification. However, the active components of the inorganic acid / MOF catalyst prepared by the traditional impregnation method are unevenly dispersed, the active components are easily lost, and the catalyst has poor reusability. Therefore, the design and preparation of reusable MOFs catalysts with excellent catalytic performance has become the focus of current research. Summary of the invention
[0004] The object of the present invention is to provide a catalyst for producing biodiesel and a preparation method thereof, so as to overcome the above-mentioned defects in the prior art.
[0005] A method for preparing a catalyst for producing biodiesel comprises the following steps:
[0006] Step (1): dissolving 1,3,5-benzenetricarboxylic acid and zirconium salt in a molar ratio of 1:1 to 6 in N,N-dimethylformamide and formic acid in a volume ratio of 1 to 2:1, ultrasonicating until the solid is dissolved, transferring the reaction solution into a reaction kettle and placing it in a drying oven for crystallization reaction, cooling, washing the crude catalyst, centrifuging and drying, and obtaining a MOF-808 catalyst;
[0007] Step (2): mixing the inorganic acid solution and the MOF-808 catalyst and placing them in a supercritical fluid, increasing the temperature and pressurizing the system to reach a supercritical condition and maintaining the condition for 1 to 10 hours, and then cooling, releasing the pressure, and unloading the kettle to obtain a crude catalyst;
[0008] Step (3): washing the crude catalyst, centrifuging and drying it to obtain the inorganic acid / MOF-808 catalyst.
[0009] Preferably, the zirconium salt in step (1) is any one of zirconium chloride, zirconium oxychloride or zirconium oxynitrate.
[0010] Preferably, in step (1), the ultrasonic condition is maintained at a power of 100 to 160 W for 5 to 60 minutes, and the crystallization reaction condition is reacted at 80 to 150° C. for 8 to 30 hours.
[0011] Preferably, the washing conditions in step (1) are 2 to 4 times of washing with 15 to 40 ml of N,N-dimethylformamide and 15 to 40 ml of ethanol each time.
[0012] Preferably, the centrifugal separation in step (1) is carried out at 3000-6000 rpm for 5-30 min, and the drying is carried out at 80-140° C. under vacuum for 4-18 h.
[0013] Preferably, in step (2), the inorganic acid is any one of phosphoric acid, sulfuric acid or hydrochloric acid, the concentration of the inorganic acid solution is 0.05-0.5 mol / l, and the mass ratio of the inorganic acid solution to MOF-808 is 0.5-5:1.
[0014] Preferably, in step (2), the supercritical fluid is any one of ethylene, carbon dioxide or nitrogen, and the supercritical conditions are a temperature of 30 to 100° C. and a pressure of 5 to 20 MPa.
[0015] Preferably, the washing conditions in step (3) are washing 2 to 4 times with 15 to 40 ml of N,N-dimethylformamide and 15 to 40 ml of ethanol each time.
[0016] Preferably, the centrifugal separation in step (3) is carried out at 3000-6000 rpm for 5-30 min, and the drying is carried out at 80-140° C. under vacuum for 4-18 h.
[0017] A catalyst used in producing biodiesel is prepared by adopting the preparation method of the catalyst used in producing biodiesel.
[0018] The beneficial effects achieved by the present invention are:
[0019] 1. The supercritical fluid of the present invention has the characteristics of high diffusivity, strong solubility, excellent surface wettability, etc. The method for preparing the inorganic acid / MOF-808 catalyst using the supercritical fluid provided by the present invention can make the inorganic acid more evenly dispersed on the MOF-808 material and have a stronger interaction with the carrier.
[0020] 2. The method of the present application is simple to operate, has a short reaction time, is easy to recycle, and the prepared inorganic acid / MOF-808 catalyst component has high dispersion uniformity, high catalytic activity, low loss rate of active components, and high reusability. The esterification reaction of oleic acid and methanol to synthesize biodiesel catalyzed by the catalyst can effectively improve the oleic acid conversion rate, inhibit the loss of active components, and improve the catalyst reusability. DETAILED DESCRIPTION
[0021] The specific implementation modes of the present invention are further explained in detail below through the description of embodiments, so as to help those skilled in the art to have a more complete, accurate and in-depth understanding of the concept and technical solution of the present invention.
[0022] The present invention provides a method for preparing a catalyst used in producing biodiesel, comprising the following steps:
[0023] Step (1): dissolving 1,3,5-benzenetricarboxylic acid and zirconium salt in N,N-dimethylformamide and formic acid, ultrasonicating until the solid is dissolved, transferring the reaction solution into a reaction kettle and placing it in a drying oven for crystallization reaction, cooling, washing the crude catalyst, centrifuging and drying, and obtaining a MOF-808 catalyst;
[0024] The zirconium salt is any one of zirconium chloride, zirconium oxychloride or zirconium oxynitrate, and the molar ratio of the zirconium salt to 1,3,5-benzenetricarboxylic acid is 1 to 6:1.
[0025] The volume ratio of N,N-dimethylformamide to formic acid is 1 to 2:1.
[0026] The ultrasonic condition is maintained at a power of 100 to 160 W for 5 to 60 minutes, preferably 30 minutes. If the power is insufficient or the ultrasonic time is insufficient, the dissolution effect is poor, which affects the crystallization and catalytic effect of the catalyst.
[0027] The crystallization reaction conditions are 80-150° C. for 8-30 hours. If the temperature is insufficient or the crystallization time is insufficient, the crystallization effect is poor, which affects the crystallization and performance of the catalyst.
[0028] In a preferred embodiment of the present invention, the washing condition is to use 15-40 ml of N,N-dimethylformamide and 15-40 ml of ethanol for 2-4 times, preferably 3 times. Insufficient washing liquid volume and insufficient washing times will result in residual impurities in the catalyst synthesis, which will not only affect the purity of the catalyst, but also affect the catalytic performance.
[0029] In a preferred embodiment of the present invention, the centrifugal separation condition is 3000-6000 rpm for 5-30 min. If the rpm is insufficient or the centrifugal time is insufficient, the separation effect is poor and the crude catalyst contains a large amount of impurities, thereby affecting the catalytic performance.
[0030] In a preferred embodiment of the present invention, the drying method is vacuum drying at 80-140° C. for 4-18 hours. If the temperature is too low or the time is too short, the solution will remain in the catalyst, which will affect the actual quality and catalytic performance of the catalyst.
[0031] Step (2): mixing the inorganic acid solution and the MOF-808 catalyst and placing them in a supercritical fluid, increasing the temperature and pressurizing the system to reach a supercritical condition and maintaining the condition for 1 to 10 hours, and then cooling, releasing the pressure, and unloading the kettle to obtain a crude catalyst;
[0032] Among them, the inorganic acid is any one of phosphoric acid, sulfuric acid or hydrochloric acid, the concentration of the inorganic acid solution is 0.05-0.5 mol / l, and the mass ratio of the inorganic acid solution to MOF-808 is 0.5-5:1. The mass ratio of the inorganic acid solution to MOF-808 is 0.5-4:1. If the amount of inorganic acid in the catalyst is too small, its catalytic effect cannot be reflected, and if the amount of inorganic acid is too much, it will exceed the solid loading limit of MOF-808, causing the inorganic acid to fall off from MOF-808 and block the MOF-808 pores. Therefore, the numerical range is selected as 0.5-5:1. The catalyst prepared within this range not only avoids the inorganic acid loading exceeding the loading limit of MOF-808, but also ensures the catalytic effect of the catalyst.
[0033] Wherein, the supercritical fluid is any one of ethylene, carbon dioxide or nitrogen, and the supercritical condition is a temperature of 30-100°C and a pressure of 5-20 MPa. Preferably, the supercritical condition is a temperature of 30-90°C and a pressure of 5-15 MPa.
[0034] Step (3): washing the crude catalyst, centrifuging and drying to obtain an inorganic acid / MOF-808 catalyst;
[0035] In a preferred embodiment of the present invention, the washing condition is to use 15-40 ml of N,N-dimethylformamide and 15-40 ml of ethanol for 2-4 times, preferably 2 times. Insufficient washing liquid volume and insufficient washing times will result in residual impurities in the catalyst synthesis, which will not only affect the purity of the catalyst, but also affect the catalytic performance.
[0036] In a preferred embodiment of the present invention, the centrifugal separation condition is 3000-6000 rpm for 5-30 min. If the rpm is insufficient or the centrifugal time is insufficient, the separation effect is poor and the crude catalyst contains a large amount of impurities, thereby affecting the catalytic performance.
[0037] In a preferred embodiment of the present invention, the drying method is vacuum drying at 80-140° C. for 4-18 hours. If the temperature is too low or the time is too short, the solution will remain in the catalyst, which will affect the actual quality and catalytic performance of the catalyst.
[0038] The present invention provides an application of the catalyst used for producing biodiesel in synthesizing biodiesel by esterification of oleic acid and methanol.
[0039] When oleic acid and methanol are esterified, oleic acid and methanol are weighed and added into a three-necked round-bottom flask, and a certain amount of inorganic acid / MOF-808 catalyst is added to perform a preparation reaction to obtain biodiesel.
[0040] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0041] Example 1
[0042] This embodiment provides a method for preparing a catalyst used in producing biodiesel, and the preparation steps are as follows:
[0043] 0.12 g of 1,3,5-benzenetricarboxylic acid and 0.8 g of zirconium chloride were dissolved in 35 ml of N,N-dimethylformamide and 35 ml of formic acid, and then ultrasonicated at 140 W for 25 min until the solid dissolved; the reaction solution was transferred into a reactor and placed in a drying oven at 120° C. for reaction for 24 h, cooled, and the resulting crude catalyst was transferred to a centrifuge tube, washed with 30 ml of N,N-dimethylformamide and 30 ml of ethanol each time, repeated washing 3 times, centrifuged at 4000 rpm for 10 min, the solid at the bottom of the centrifuge tube was collected, transferred to a vacuum drying oven and dried at 100° C. for 12 h to obtain a MOF-808 catalyst.
[0044] In a reactor, 0.4g MOF-808 catalyst was immersed in 40ml of 0.05mol / l sulfuric acid solution, and the temperature in the reactor was raised to 60℃ by program temperature increase, and then carbon dioxide gas was charged into the reactor by a high-pressure injection pump to make the pressure in the reactor reach 9MPa to achieve supercritical conditions, and then the supercritical conditions were maintained for 5h. After the supercritical treatment was completed, the reactor was cooled, depressurized, and unloaded to obtain a crude catalyst. The obtained crude catalyst was transferred to a centrifuge tube, washed with 30ml N,N-dimethylformamide and 30ml ethanol each time, and the washing was repeated twice, centrifuged at 4000 rpm for 10min, and the solid at the bottom of the centrifuge tube was collected and transferred to a vacuum drying oven and dried at 100℃ for 12h to obtain an inorganic acid / MOF-808 catalyst.
[0045] Example 2
[0046] This embodiment provides a method for preparing a catalyst used in producing biodiesel, and the preparation steps are as follows:
[0047] 0.25 g of 1,3,5-benzenetricarboxylic acid and 1.06 g of zirconium oxychloride were dissolved in 30 ml of N,N-dimethylformamide and 30 ml of formic acid, and then ultrasonicated at 120 W for 30 min until the solid dissolved; the reaction solution was transferred into a reactor and placed in a drying oven at 130° C. for reaction for 20 h, cooled, and the obtained crude catalyst was transferred to a centrifuge tube, and washed with 40 ml of N,N-dimethylformamide and 40 ml of ethanol each time, repeated washing twice, and centrifuged at 5000 rpm for 15 min. The solid at the bottom of the centrifuge tube was collected, transferred to a vacuum drying oven and dried at 120° C. for 8 h to obtain a MOF-808 catalyst.
[0048] In a reactor, 0.35g MOF-808 catalyst was immersed in 35ml of 0.1mol / l phosphoric acid solution, and the temperature in the reactor was raised to 70°C by program temperature increase, and then nitrogen gas was filled into the reactor by a high-pressure injection pump to make the pressure in the reactor reach 12MPa to achieve supercritical conditions, and then the supercritical conditions were maintained for 6h. After the supercritical treatment was completed, the reactor was cooled, depressurized, and unloaded to obtain a crude catalyst. The obtained crude catalyst was transferred to a centrifuge tube, washed with 40ml N,N-dimethylformamide and 40ml ethanol each time, and the washing was repeated twice, centrifuged at 5000 rpm for 15min, and the solid at the bottom of the centrifuge tube was collected and transferred to a vacuum drying oven and dried at 120°C for 8h to obtain an inorganic acid / MOF-808 catalyst.
[0049] Example 3
[0050] This embodiment provides a method for preparing a catalyst used in producing biodiesel, and the preparation steps are as follows:
[0051] 0.18 g of 1,3,5-benzenetricarboxylic acid and 0.94 g of zirconium oxynitrate were dissolved in 30 ml of N,N-dimethylformamide and 30 ml of formic acid, and then ultrasonicated at 150 W for 35 min until the solid dissolved; the reaction solution was transferred into a reactor and placed in a drying oven at 120° C. for reaction for 18 h, cooled, and the resulting crude catalyst was transferred to a centrifuge tube, washed with 35 ml of N,N-dimethylformamide and 35 ml of ethanol each time, repeated washing 3 times, centrifuged at 6000 rpm for 10 min, the solid at the bottom of the centrifuge tube was collected, transferred to a vacuum drying oven and dried at 130° C. for 12 h to obtain a MOF-808 catalyst.
[0052] In a reactor, 0.3g MOF-808 catalyst was immersed in 30ml of 0.2mol / l hydrochloric acid solution, and the temperature in the reactor was raised to 65°C by program heating, and then ethylene gas was charged into the reactor by a high-pressure injection pump to make the pressure in the reactor reach 10MPa to achieve supercritical conditions, and then the supercritical conditions were maintained for 5h. After the supercritical treatment was completed, the reactor was cooled, depressurized, and unloaded to obtain a crude catalyst. The obtained crude catalyst was transferred to a centrifuge tube, washed with 35ml N,N-dimethylformamide and 35ml ethanol each time, and the washing was repeated 3 times, centrifuged at 6000 rpm for 10min, and the solid at the bottom of the centrifuge tube was collected and transferred to a vacuum drying oven and dried at 130°C for 12h to obtain an inorganic acid / MOF-808 catalyst.
[0053] Example 4
[0054] This embodiment provides a method for preparing a catalyst used in producing biodiesel, and the preparation steps are as follows:
[0055] 0.32 g of 1,3,5-benzenetricarboxylic acid and 1.25 g of zirconium oxychloride were dissolved in 40 ml of N,N-dimethylformamide and 40 ml of formic acid, and then ultrasonicated at 140 W for 30 min until the solid dissolved; the reaction solution was transferred into a reactor and placed in a drying oven at 130° C. for reaction for 24 h, cooled, and the obtained crude catalyst was transferred to a centrifuge tube, and washed with 40 ml of N,N-dimethylformamide and 40 ml of ethanol each time, repeated washing 3 times, centrifuged at 6000 rpm for 10 min, and the solid at the bottom of the centrifuge tube was collected and transferred to a vacuum drying oven and dried at 120° C. for 12 h to obtain a MOF-808 catalyst.
[0056] In a reactor, 0.5g MOF-808 catalyst was immersed in 50ml of 0.1mol / l sulfuric acid solution, and the temperature in the reactor was raised to 70℃ by program temperature increase. Then, carbon dioxide gas was charged into the reactor by a high-pressure injection pump to make the pressure in the reactor reach 12MPa to achieve supercritical conditions, and then the supercritical conditions were maintained for 6h. After the supercritical treatment was completed, the reactor was cooled, depressurized, and unloaded to obtain a crude catalyst. The obtained crude catalyst was transferred to a centrifuge tube, washed with 40ml N,N-dimethylformamide and 40ml ethanol each time, and washed twice, centrifuged at 6000 rpm for 15min, and the solid at the bottom of the centrifuge tube was collected and transferred to a vacuum drying oven and dried at 120℃ for 12h to obtain an inorganic acid / MOF-808 catalyst.
[0057] Example 5
[0058] This embodiment provides a method for preparing a catalyst used in producing biodiesel, and the preparation steps are as follows:
[0059] 0.40 g of 1,3,5-benzenetricarboxylic acid and 1.32 g of zirconium chloride were dissolved in 50 ml of N,N-dimethylformamide and 40 ml of formic acid, and then ultrasonicated at 160 W for 40 min until the solid dissolved; the reaction solution was transferred into a reactor and placed in a drying oven at 140° C. for reaction for 18 h, cooled, and the resulting crude catalyst was transferred to a centrifuge tube, washed with 40 ml of N,N-dimethylformamide and 40 ml of ethanol each time, repeated washing 3 times, centrifuged at 4000 rpm for 25 min, the solid at the bottom of the centrifuge tube was collected, transferred to a vacuum drying oven and dried at 140° C. for 12 h to obtain a MOF-808 catalyst.
[0060] In a reactor, 0.4g MOF-808 catalyst was immersed in 45ml of 0.15mol / l phosphoric acid solution, and the temperature in the reactor was raised to 75°C by program temperature increase, and then nitrogen gas was filled into the reactor by a high-pressure injection pump to make the pressure in the reactor reach 12MPa to achieve supercritical conditions, and then the supercritical conditions were maintained for 7h. After the supercritical treatment was completed, the reactor was cooled, depressurized, and unloaded to obtain a crude catalyst. The obtained crude catalyst was transferred to a centrifuge tube, washed with 40ml N,N-dimethylformamide and 40ml ethanol each time, and the washing was repeated twice, centrifuged at 4000 rpm for 25min, and the solid at the bottom of the centrifuge tube was collected and transferred to a vacuum drying oven and dried at 140°C for 12h to obtain an inorganic acid / MOF-808 catalyst.
[0061] Example 6
[0062] This embodiment provides a method for preparing a catalyst used in producing biodiesel, and the preparation steps are as follows:
[0063] 0.35 g of 1,3,5-benzenetricarboxylic acid and 1.28 g of zirconium chloride were dissolved in 40 ml of N,N-dimethylformamide and 40 ml of formic acid, and then ultrasonicated at 140 W for 25 min until the solid dissolved; the reaction solution was transferred into a reactor and placed in a drying oven at 120° C. for reaction for 24 h, cooled, and the resulting crude catalyst was transferred to a centrifuge tube, washed with 35 ml of N,N-dimethylformamide and 35 ml of ethanol each time, repeated washing twice, and centrifuged at 5000 rpm for 20 min. The solid at the bottom of the centrifuge tube was collected, transferred to a vacuum drying oven, and dried at 130° C. for 8 h to obtain a MOF-808 catalyst.
[0064] In a reactor, 0.4g MOF-808 catalyst was immersed in 45ml of 0.2mol / l sulfuric acid solution, and the temperature in the reactor was raised to 65°C by program heating, and then carbon dioxide gas was charged into the reactor by a high-pressure injection pump to make the pressure in the reactor reach 9MPa to achieve supercritical conditions, and then the supercritical conditions were maintained for 5h. After the supercritical treatment was completed, the reactor was cooled, depressurized, and unloaded to obtain a crude catalyst. The obtained crude catalyst was transferred to a centrifuge tube, washed with 35ml N,N-dimethylformamide and 35ml ethanol each time, and the washing was repeated twice, centrifuged at 5000 rpm for 20min, and the solid at the bottom of the centrifuge tube was collected and transferred to a vacuum drying oven and dried at 130°C for 8h to obtain an inorganic acid / MOF-808 catalyst.
[0065] Comparative Example 1
[0066] This embodiment provides an inorganic acid / MOF-808 catalyst prepared by a traditional impregnation method, and the preparation steps are as follows:
[0067] 0.12 g of 1,3,5-benzenetricarboxylic acid and 0.8 g of zirconium chloride were dissolved in 35 ml of N,N-dimethylformamide and 35 ml of formic acid, and then ultrasonicated at 140 W for 25 min until the solid dissolved; the reaction solution was transferred into a reactor and placed in a drying oven at 120° C. for reaction for 24 h, cooled, and the resulting crude catalyst was transferred to a centrifuge tube, washed with 30 ml of N,N-dimethylformamide and 30 ml of ethanol each time, repeated washing 3 times, centrifuged at 4000 rpm for 10 min, the solid at the bottom of the centrifuge tube was collected, transferred to a vacuum drying oven and dried at 100° C. for 12 h to obtain a MOF-808 catalyst.
[0068] In a reactor, 0.4 g of MOF-808 catalyst was immersed in 40 ml of 0.05 mol / l sulfuric acid solution and stirred for 24 h. The crude catalyst was transferred to a centrifuge tube and washed with 30 ml of N,N-dimethylformamide and 30 ml of ethanol each time. The washing was repeated twice and centrifuged at 4000 rpm for 10 min. The solid at the bottom of the centrifuge tube was collected and transferred to a vacuum drying oven and dried at 100 °C for 12 h to obtain an inorganic acid / MOF-808 catalyst.
[0069] Comparative Example 2
[0070] This embodiment provides an inorganic acid / MOF-808 catalyst prepared by a traditional impregnation method, and the preparation steps are as follows:
[0071] 0.25 g of 1,3,5-benzenetricarboxylic acid and 1.06 g of zirconium oxychloride were dissolved in 30 ml of N,N-dimethylformamide and 30 ml of formic acid, and then ultrasonicated at 120 W for 30 min until the solid dissolved; the reaction solution was transferred into a reactor and placed in a drying oven at 130° C. for reaction for 20 h, cooled, and the obtained crude catalyst was transferred to a centrifuge tube, and washed with 40 ml of N,N-dimethylformamide and 40 ml of ethanol each time, repeated washing twice, and centrifuged at 5000 rpm for 15 min. The solid at the bottom of the centrifuge tube was collected, transferred to a vacuum drying oven and dried at 120° C. for 8 h to obtain a MOF-808 catalyst.
[0072] In a reactor, 0.35 g of MOF-808 catalyst was immersed in 35 ml of 0.1 mol / l phosphoric acid solution and stirred for 24 h. The crude catalyst was transferred to a centrifuge tube and washed with 40 ml of N,N-dimethylformamide and 40 ml of ethanol each time. The washing was repeated twice and centrifuged at 5000 rpm for 15 min. The solid at the bottom of the centrifuge tube was collected and transferred to a vacuum drying oven and dried at 120 ° C for 8 h to obtain an inorganic acid / MOF-808 catalyst.
[0073] Application Examples
[0074] Add 12ml methanol and 6ml oleic acid to a round-bottom flask, put in a magnetic rotor (set speed 600r / min) and place in an oil bath for reaction, reflux condensation, and when the temperature reaches 75°C, add 0.38g of inorganic acid / MOF-808 catalyst. After 5h of reaction, take an appropriate amount of reactants and centrifuge to separate the catalyst. After each reaction, the catalyst is centrifuged, washed and dried for reuse. And test various indicators of the reaction.
[0075] 1. Determine the acid value of the solution according to the method described in GB / T1668-2008 "Determination of Acid Value and Acidity of Plasticizers". Calculate the conversion rate of oleic acid by measuring the acid value of the solution before and after the reaction. Conversion rate of oleic acid = (acid value of the solution before the reaction - acid value of the solution after the reaction) / acid value of the solution before the reaction. The test results are shown in Table 1;
[0076] 2. The ICP method was used to measure the amount of S, P or Cl A in the inorganic acid / MOF-808 catalyst before the reaction. After repeated use for 4 times, the ICP method was used to determine the amount of S, P or Cl B in the inorganic acid / MOF-808 catalyst. Then the inorganic acid was calculated according to the following formula
[0077] / The active component loss rate of MOF-808 catalyst, active component loss rate = (AB) / A*100%, the calculation results are shown in Table 1.
[0078] Table 1 Test results of various indicators of esterification reaction of oleic acid and methanol
[0079]
[0080]
[0081] As can be seen from Table 1, the inorganic acid / MOF-808 catalyst prepared by the method of Examples 1-6 of the present invention has a better catalytic reaction effect than the inorganic acid / MOF-808 catalyst prepared by the traditional impregnation method (Comparative Examples 1-2). Specifically, in the reaction of esterification of oleic acid and methanol to prepare biodiesel, the oleic acid conversion rate of the inorganic acid / MOF-808 provided by Examples 1-6 of the present invention after the first use and repeated use for 4 times is significantly better than that of the inorganic acid / MOF-808 catalyst prepared by the traditional impregnation method (Comparative Examples 1-2).
[0082] By measuring the loss rate of active components of the inorganic acid / MOF-808 catalyst after being reused 4 times, we found that the inorganic acid / MOF-808 catalyst provided in the embodiment of the present invention has a low loss rate of active components after being reused 4 times, so that the catalyst can maintain its catalytic activity for the esterification reaction of oleic acid and methanol to prepare biodiesel for a long time.
[0083] In summary, the inorganic acid / MOF-808 catalyst prepared by the supercritical fluid provided by the present invention exhibits good activity in the catalytic esterification of oleic acid and methanol to prepare biodiesel, and the catalyst has a low loss rate of active components and high reusability. It is particularly pointed out that the method for preparing the catalyst under supercritical fluid is simple to operate, has a short reaction time, and the active components are evenly dispersed. This lays a foundation for the industrialization of the method.
[0084] The above-described embodiments of the present invention do not constitute a limitation on the protection scope of the present invention. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a catalyst for producing biodiesel, characterized in that: The steps include: Step (1): dissolving 1,3,5-benzenetricarboxylic acid and zirconium salt in a molar ratio of 1:1 to 6 in N,N-dimethylformamide and formic acid in a volume ratio of 1 to 2:1, ultrasonicating until the solid is dissolved, transferring the reaction solution into a reaction kettle and placing it in a drying oven for crystallization reaction, cooling, washing the crude catalyst, centrifuging and drying, and obtaining a MOF-808 catalyst; Step (2): mixing the inorganic acid solution and the MOF-808 catalyst and placing them in a supercritical fluid, increasing the temperature and pressurizing the system to reach a supercritical condition and maintaining the condition for 1 to 10 hours, and then cooling, releasing the pressure, and unloading the kettle to obtain a crude catalyst; Step (3): washing the crude catalyst, centrifuging and drying it to obtain the inorganic acid / MOF-808 catalyst.
2. The method for preparing a catalyst for producing biodiesel according to claim 1, characterized in that: The zirconium salt in step (1) is any one of zirconium chloride, zirconium oxychloride or zirconium oxynitrate.
3. The method for preparing a catalyst for producing biodiesel according to claim 1, characterized in that: In step (1), the ultrasonic condition is maintained at a power of 100 to 160 W for 5 to 60 minutes, and the crystallization reaction condition is reacted at 80 to 150° C. for 8 to 30 hours.
4. The method for preparing a catalyst for producing biodiesel according to claim 1, characterized in that: The washing conditions in step (1) are 2 to 4 times of washing with 15 to 40 ml of N,N-dimethylformamide and 15 to 40 ml of ethanol each time.
5. The method for preparing a catalyst for producing biodiesel according to claim 1, characterized in that: The centrifugal separation conditions in step (1) are centrifugation at 3000-6000 rpm for 5-30 min, and the drying conditions are vacuum drying at 80-140° C. for 4-18 h.
6. The method for preparing a catalyst for producing biodiesel according to claim 1, characterized in that: In step (2), the inorganic acid is any one of phosphoric acid, sulfuric acid or hydrochloric acid, the concentration of the inorganic acid solution is 0.05-0.5 mol / l, and the mass ratio of the inorganic acid solution to MOF-808 is 0.5-5:
1.
7. The method for preparing a catalyst for producing biodiesel according to claim 1, characterized in that: In step (2), the supercritical fluid is any one of ethylene, carbon dioxide or nitrogen, and the supercritical conditions are a temperature of 30 to 100° C. and a pressure of 5 to 20 MPa.
8. The method for preparing a catalyst for producing biodiesel according to claim 1, characterized in that: The washing conditions in step (3) are washing 2 to 4 times with 15 to 40 ml of N,N-dimethylformamide and 15 to 40 ml of ethanol each time.
9. The method for preparing a catalyst for producing biodiesel according to claim 1, characterized in that: The centrifugal separation conditions in step (3) are centrifugation at 3000-6000 rpm for 5-30 min, and the drying conditions are vacuum drying at 80-140° C. for 4-18 h.
10. A catalyst for producing biodiesel, characterized in that: The catalyst is prepared by the method for preparing the catalyst for producing biodiesel as described in any one of claims 1 to 9.