Responsive Janus cage catalyst as well as preparation method and application thereof
Through the design of responsive Janus cage-shaped catalyst, the problem of catalysis and separation of Janus materials in aqueous solvents is solved by using sulfonated polystyrene spheres, magnetic cages and temperature-sensitive polymers to support gold nanoparticles, and high efficiency is achieved Catalytic and environmentally friendly catalytic reactions reduce environmental pollution.
Patent Information
- Application Number
- CN202411081126.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-26
AI Technical Summary
The existing Janus materials need to use organic solvents to separate product in phase transfer catalytic system, resulting in environmental pollution and low catalytic efficiency, and lack of solutions for efficient catalytic in aqueous solvents.
Design a responsive Janus cage-shaped catalyst, through the preparation of sulfonated polystyrene spheres, magnetic cages and temperature-sensitive polymer grafting, gold nanoparticles are supported, catalytic and magnetic separation is achieved, and the target substance is used to use temperature responsiveness. Enrichment and controlled release.
It realizes the separation and controllable release of highly efficient catalytic reaction products in aqueous solvents, reduces environmental pollution, improves catalytic efficiency, and has multiple responsiveness, which is suitable for the enrichment and release of oil-soluble substances.
Smart Images

Figure CN119016111A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a responsive Janus cage catalyst and a preparation method and application thereof. Background Art
[0002] As a new type of material, Janus materials have potential application prospects in many important fields due to their unique structure and composition, and have gradually become a research hotspot in the field of new materials science. In 1991, French scientist PG de Gennes gave a detailed introduction to Janus particles in his Nobel Prize speech, which aroused widespread attention from scientific researchers to Janus materials. Janus particles refer to particles with chemical asymmetry, which can give Janus particles two different or even opposite properties, such as polarity / non-polarity, hydrophilicity / hydrophobicity, anion / cation, uncharged / charged, etc. The shapes of Janus particles are also diverse, from simple spherical Janus particles to different types of non-spherical Janus particles, from Janus sheets and Janus tubes with highly anisotropic structures to three-dimensional Janus hollow spheres.
[0003] The morphology and chemical composition of Janus materials have a crucial impact on their performance. Janus nanosheets (disks) with two-dimensional structures can act as particle emulsifiers to emulsify oil / water phases when the two sides are modified with hydrophilic groups and lipophilic groups respectively. Because their two-dimensional sheet structures have stronger anisotropy, they are more difficult to flip at the emulsion interface, so a more stable emulsion can be obtained. Different chemical compositions can give Janus materials more unique properties and potential applications. Grafting catalytically active materials (such as PW) on one side of the Janus nanosheet can improve the performance of Janus materials. 12 O 40 3- ), using it as a particle emulsifier to emulsify the oil / water phases, catalyzing the catalytic oxidative degradation of azo dyes (such as methyl orange) in the water phase in the emulsion system, and the dye molecules are catalytically degraded at the emulsion interface, and some of the degradation intermediates (such as methylaniline, dimethylaniline, etc.) tend to be more oil-soluble, and therefore are extracted into the oil phase. This catalytic system not only increases the catalytic interface, but also the intermediates are extracted into the oil phase as the reaction proceeds, so that the synergistic effect of interfacial catalysis and phase transfer greatly improves the catalytic efficiency.
[0004] Although the feasibility of Janus materials in phase transfer catalysis has been proven, the system still requires organic solvents as the extraction phase for product separation, and the environmental pollution caused by the large-scale use of organic solvents is also an urgent problem to be solved. Water, as an environmentally friendly chemical reaction medium, has attracted widespread attention. Using green solvent water to replace toxic and harmful organic solvents has important environmental significance. Therefore, it is very important to design and prepare a catalyst with high catalytic performance in water solvent, and it is also very critical to achieve simple separation of products. Summary of the invention
[0005] The purpose of the present invention is to provide a responsive Janus cage catalyst and a preparation method and application thereof, which has both catalytic and separation properties and is easy to recycle.
[0006] The technical solution of the present invention is achieved in this way:
[0007] The present invention provides a method for preparing a responsive Janus cage catalyst, comprising the following steps:
[0008] S1. Preparation of sulfonated polystyrene spheres: polystyrene spheres are mixed with concentrated sulfuric acid, reacted for 1-6 hours, the reaction mixture is dripped into water, filtered, washed several times until the filtrate is neutral, and vacuum dried to obtain sulfonated polystyrene spheres;
[0009] Preparation of S2.PS@Fe3O4 balls: Disperse the dried sulfonated polystyrene balls in water, introduce nitrogen to remove oxygen in the system, add ferric chloride and ferrous chloride, stir for 12-24 hours, filter, disperse again in deoxygenated water, add NaOH aqueous solution, adjust the pH to 10-12, react for 1-3 hours, filter, wash several times until the filtrate is neutral, and vacuum dry to obtain PS@Fe3O4 balls;
[0010] S3. Preparation of inorganic magnetic cages: PS@Fe3O4 balls were dispersed in ethanol, tetraethyl orthosilicate was added, ammonia water was added, the reaction was stirred for 3-6 hours, and centrifuged to wash to obtain PS@Fe3O4@SiO2 balls, and an organic solvent was added to remove polystyrene to obtain Fe3O4@SiO2 inorganic magnetic cages;
[0011] S4. Preparation of responsive Janus cage: disperse Fe3O4@SiO2 inorganic magnetic cage in water, add initiator, stir for 1-3h, filter, disperse in water again, add monomer of thermosensitive polymer, react at 60-80℃ for 6-12h, separate by magnetic separation, wash, dry, and obtain temperature responsive Janus cage;
[0012] S5. Preparation of responsive Janus cage catalyst: disperse the temperature-responsive Janus cage in water, add chloroauric acid, stir for 1-3 hours, filter, disperse in water again, add sodium borohydride, react for 1-2 hours, and obtain a responsive Janus cage catalyst loaded with gold nanoparticles.
[0013] As a further improvement of the present invention, in step S1, the polystyrene balls are linear polystyrene balls, and the mass ratio of the polystyrene balls to concentrated sulfuric acid is 1:5-20.
[0014] As a further improvement of the present invention, in step S2, the molar ratio of ferric chloride to ferrous chloride is 1:1, and the mass ratio of the sulfonated polystyrene balls to ferric chloride is 1:5-20.
[0015] As a further improvement of the present invention, in step S3, the mass ratio of PS@Fe3O4 balls, ethanol and tetraethyl orthosilicate is 1:20-30:4-8, the concentration of ammonia water added is 2-5wt%, and the organic solvent added is a good solvent for polystyrene.
[0016] As a further improvement of the present invention, in step S3, the organic solvent is selected from one of toluene, dimethylformamide, dimethylacetamide, chloroform and tetrahydrofuran.
[0017] As a further improvement of the present invention, in step S4, the initiator is a carboxyl-containing initiator, preferably azobiscyanovaleric acid; the mass ratio of Fe3O4@SiO2 inorganic magnetic cage to the initiator is 1:1-3.
[0018] As a further improvement of the present invention, in step S4, the monomer of the thermosensitive polymer is selected from one of N-isopropyl acrylamide, N,N-diethyl acrylamide, N-(L)-(1-hydroxymethyl)propyl methacrylamide, and N-acryloyloxy-N-alkylpiperazine; the mass of the monomer of the thermosensitive polymer is 3-5 times the mass of the Fe3O4@SiO2 inorganic magnetic cage.
[0019] As a further improvement of the present invention, in step S5, the mass of the chloroauric acid is 0.1-1 times the mass of the temperature-responsive Janus cage, and the mass of the sodium borohydride is 0.1-0.5 times the mass of the temperature-responsive Janus cage.
[0020] The present invention further protects a responsive Janus cage catalyst prepared by the above preparation method.
[0021] The present invention further protects the use of a responsive Janus cage catalyst prepared by the above preparation method in phase transfer catalysis.
[0022] The basic principles of the present invention are as follows:
[0023] (1) After the polystyrene spheres are sulfonated, sulfonate groups are introduced on the surface of the spheres. The sulfonate groups adsorb ferric ions and ferrous ions. After adding sodium hydroxide, ferrosoferric oxide is obtained, thereby obtaining magnetic PS@Fe3O4 spheres.
[0024] (2) TEOS further undergoes a sol-gel reaction on the surface of the PS@Fe3O4 spheres, coating the surface of the microspheres with a layer of silica. At the same time, the reaction in an alkaline environment causes the silica layer to have a porous structure.
[0025] (3) The linear polystyrene spheres are removed by organic solvent to obtain Fe3O4@SiO2 hollow spheres, with the inner layer being Fe3O4 and the outer layer being SiO2, i.e., a magnetic Janus cage. By taking advantage of the different chemical properties of ferroferric oxide and silicon dioxide, the carboxyl-containing initiator can coordinate with iron and adsorb on the inner layer Fe3O4. Then, the carboxyl-containing initiator induces the monomers of the thermosensitive polymer to polymerize in the inner layer, thus obtaining a Janus cage with the inner layer grafted with the thermosensitive polymer.
[0026] (4) By utilizing the coordination effect between the nitrogen element and the metal in the responsive polymer, Au particles are loaded to obtain a composite Janus cage with both temperature responsiveness and catalytic function.
[0027] The present invention has the following beneficial effects: the Janus cage catalyst prepared by the present invention has multiple responsiveness such as catalysis, magnetic separation, temperature response, etc., and can be used to achieve enrichment and controllable release of target substances. When the ambient temperature is higher than the LCST of the thermosensitive, the cage becomes hydrophobic and can be used to enrich oil-soluble substances from the water environment; when the ambient temperature is lower than its LCST, the thermosensitive polymer becomes hydrophilic and can achieve controllable release of oil-soluble substances. The separation of the catalytic reaction product from the reaction system and further controllable release are achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0029] Figure 1 This is the TEM image of the responsive Janus cage catalyst prepared in Example 1 of the present invention.
[0030] Figure 2This is the infrared spectrum of Fe3O4@SiO2 inorganic magnetic cage before and after grafting thermosensitive polymer poly N-isopropylacrylamide in Example 1 of the present invention, curve 1 is before grafting, and curve 2 is after grafting. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] This embodiment provides a method for preparing a responsive Janus cage catalyst, comprising the following steps:
[0034] S1. Preparation of sulfonated polystyrene spheres: 1 g of linear polystyrene spheres was mixed with 20 g of concentrated sulfuric acid, and the reaction mixture was added dropwise to water after 1 h of reaction, filtered, washed several times until the filtrate was neutral, and vacuum dried to obtain sulfonated polystyrene spheres;
[0035] Preparation of S2.PS@Fe3O4 balls: 0.1 g of dried sulfonated polystyrene balls were dispersed in 10 g of water, nitrogen was introduced to remove oxygen in the system, 1 g of ferric chloride and 0.78 g of ferrous chloride were added, stirred for 24 h, filtered, dispersed again in deoxygenated water, NaOH aqueous solution was added, pH was adjusted to 12, reacted for 1 h, filtered, washed several times until the filtrate was neutral, and vacuum dried to obtain PS@Fe3O4 balls;
[0036] S3. Preparation of inorganic magnetic cages: 0.1 g PS@Fe3O4 balls were dispersed in 20 g ethanol, 0.4 g ethyl orthosilicate and 0.4 g ammonia were added, the mixture was stirred for 6 h, and centrifuged to obtain PS@Fe3O4@SiO2 balls. A large amount of organic solvent dimethylformamide was added to remove polystyrene to obtain Fe3O4@SiO2 inorganic magnetic cages.
[0037] S4. Preparation of responsive Janus cage: 0.1g Fe3O4@SiO2 inorganic magnetic cage was dispersed in 10ml water, 0.1g azobiscyanovaleric acid was added as initiator, stirred for 3h, filtered, dispersed in water again, 0.3g N-isopropylacrylamide, a monomer of thermosensitive polymer, was added, reacted at 80℃ for 6h, magnetically separated, washed, and dried to obtain temperature-responsive Janus cage;
[0038] S5. Preparation of responsive Janus cage catalyst: Disperse 0.1 g of temperature-responsive Janus cage in 10 ml of water, add 0.05 g of chloroauric acid, stir for 3 h, filter, disperse in water again, add 0.05 g of sodium borohydride, react for 1 h, and obtain a responsive Janus cage catalyst loaded with gold nanoparticles.
[0039] TEM of Janus cage catalysts Figure 1 As shown in the figure, it can be seen that it is a hollow structure with holes in the shell. The successful grafting of the thermosensitive polymer poly N-isopropylacrylamide (PNIPAM) inside the shell can be proved by infrared spectroscopy. The results are shown in Figure 2 As shown in the figure, curve 1 is the Fe3O4@SiO2 inorganic magnetic cage without PNIPAM grafting, and curve 2 is the temperature-responsive Janus cage obtained after Fe3O4@SiO2 inorganic magnetic cage grafted with PNIPAM. By comparison, it can be found that after grafting PNIPAM, 1544cm -1 and 1658cm -1 The characteristic peak of PNIPAM appeared, proving the successful grafting of PNIPAM.
[0040] Comparative Example 1: The difference between Comparative Example 1 and Example 1 is that the monomer N-isopropylacrylamide of the thermosensitive polymer is not added.
[0041] Comparative Example 2: This comparative example differs from Example 1 only in that azobisisobutylamidine hydrochloride is used as the initiator instead of azobiscyanovaleric acid.
[0042] Comparative Example 3: This comparative example differs from Example 1 only in that ethyl orthosilicate is not added.
[0043] Example 2
[0044] This embodiment provides a method for preparing a responsive Janus cage catalyst, comprising the following steps:
[0045] S1. Preparation of sulfonated polystyrene spheres: 1 g of linear polystyrene spheres was mixed with 20 g of concentrated sulfuric acid, and the reaction mixture was added dropwise to water after 1 h of reaction, filtered, washed several times until the filtrate was neutral, and vacuum dried to obtain sulfonated polystyrene spheres;
[0046] Preparation of S2.PS@Fe3O4 balls: 0.1 g of dried sulfonated polystyrene balls were dispersed in 10 g of water, nitrogen was introduced to remove oxygen in the system, 1 g of ferric chloride and 0.78 g of ferrous chloride were added, stirred for 24 h, filtered, dispersed again in deoxygenated water, NaOH aqueous solution was added, pH was adjusted to 12, reacted for 1 h, filtered, washed several times until the filtrate was neutral, and vacuum dried to obtain PS@Fe3O4 balls;
[0047] S3. Preparation of inorganic magnetic cages: 0.1 g PS@Fe3O4 balls were dispersed in 20 g ethanol, 0.4 g ethyl orthosilicate and 0.4 g ammonia were added, the mixture was stirred for 6 h, and centrifuged to obtain PS@Fe3O4@SiO2 balls. A large amount of organic solvent dimethylformamide was added to remove polystyrene to obtain Fe3O4@SiO2 inorganic magnetic cages.
[0048] S4. Preparation of responsive Janus cage: 0.1g Fe3O4@SiO2 inorganic magnetic cage was dispersed in 10ml water, 0.1g azobiscyanovaleric acid initiator was added, stirred for 3h, filtered, dispersed in water again, 0.3g N-(L)-(1-hydroxymethyl)propyl methacrylamide, a monomer of thermosensitive polymer, was added, reacted at 60℃ for 8h, magnetically separated, washed, and dried to obtain temperature-responsive Janus cage;
[0049] S5. Preparation of responsive Janus cage catalyst: Disperse 0.1 g of temperature-responsive Janus cage in 10 ml of water, add 0.05 g of chloroauric acid, stir for 3 h, filter, disperse in water again, add 0.05 g of sodium borohydride, react for 1 h, and obtain a responsive Janus cage catalyst loaded with gold nanoparticles.
[0050] Example 3
[0051] This embodiment provides a method for preparing a responsive Janus cage catalyst, comprising the following steps:
[0052] S1. Preparation of sulfonated polystyrene spheres: 1 g of linear polystyrene spheres was mixed with 20 g of concentrated sulfuric acid, and the reaction mixture was added dropwise to water after 1 h of reaction, filtered, washed several times until the filtrate was neutral, and vacuum dried to obtain sulfonated polystyrene spheres;
[0053] Preparation of S2.PS@Fe3O4 balls: 0.1 g of dried sulfonated polystyrene balls were dispersed in 10 g of water, nitrogen was introduced to remove oxygen in the system, 1 g of ferric chloride and 0.78 g of ferrous chloride were added, stirred for 24 h, filtered, dispersed again in deoxygenated water, NaOH aqueous solution was added, pH was adjusted to 12, reacted for 1 h, filtered, washed several times until the filtrate was neutral, and vacuum dried to obtain PS@Fe3O4 balls;
[0054] S3. Preparation of inorganic magnetic cages: 0.1 g PS@Fe3O4 balls were dispersed in 20 g ethanol, 0.4 g ethyl orthosilicate and 0.4 g ammonia were added, the mixture was stirred for 6 h, and centrifuged to obtain PS@Fe3O4@SiO2 balls. A large amount of organic solvent dimethylformamide was added to remove polystyrene to obtain Fe3O4@SiO2 inorganic magnetic cages.
[0055] S4. Preparation of responsive Janus cage: 0.1g Fe3O4@SiO2 inorganic magnetic cage was dispersed in 10ml water, 0.1g azobiscyanovaleric acid was added as initiator, stirred for 3h, filtered, dispersed in water again, 0.3g N,N-diethylacrylamide, a monomer of thermosensitive polymer, was added, reacted at 80℃ for 6h, magnetically separated, washed, and dried to obtain temperature-responsive Janus cage;
[0056] S5. Preparation of responsive Janus cage catalyst: Disperse 0.1 g of temperature-responsive Janus cage in 10 ml of water, add 0.05 g of chloroauric acid, stir for 3 h, filter, disperse in water again, add 0.05 g of sodium borohydride, react for 1 h, and obtain a responsive Janus cage catalyst loaded with gold nanoparticles.
[0057] Example 4
[0058] This embodiment provides a method for preparing a responsive Janus cage catalyst, comprising the following steps:
[0059] S1. Preparation of sulfonated polystyrene spheres: 1 g of linear polystyrene spheres was mixed with 20 g of concentrated sulfuric acid, and the reaction mixture was added dropwise to water after 1 h of reaction, filtered, washed several times until the filtrate was neutral, and vacuum dried to obtain sulfonated polystyrene spheres;
[0060] Preparation of S2.PS@Fe3O4 balls: 0.1 g of dried sulfonated polystyrene balls were dispersed in 10 g of water, nitrogen was introduced to remove oxygen in the system, 1 g of ferric chloride and 0.78 g of ferrous chloride were added, stirred for 24 h, filtered, dispersed again in deoxygenated water, NaOH aqueous solution was added, pH was adjusted to 12, reacted for 1 h, filtered, washed several times until the filtrate was neutral, and vacuum dried to obtain PS@Fe3O4 balls;
[0061] S3. Preparation of inorganic magnetic cages: 0.1 g PS@Fe3O4 balls were dispersed in 20 g ethanol, 0.4 g ethyl orthosilicate and 0.4 g ammonia were added, the mixture was stirred for 6 h, and centrifuged to obtain PS@Fe3O4@SiO2 balls. A large amount of organic solvent dimethylformamide was added to remove polystyrene to obtain Fe3O4@SiO2 inorganic magnetic cages.
[0062] S4. Preparation of responsive Janus cage: 0.1g Fe3O4@SiO2 inorganic magnetic cage was dispersed in 10ml water, 0.1g azobiscyanovaleric acid was added as initiator, stirred for 3h, filtered, dispersed in water again, 0.3g N-acryloyloxy-N-alkylpiperazine, a monomer of thermosensitive polymer, was added, reacted at 80℃ for 6h, magnetically separated, washed, and dried to obtain temperature-responsive Janus cage;
[0063] S5. Preparation of responsive Janus cage catalyst: Disperse 0.1 g of temperature-responsive Janus cage in 10 ml of water, add 0.05 g of chloroauric acid, stir for 3 h, filter, disperse in water again, add 0.05 g of sodium borohydride, react for 1 h, and obtain a responsive Janus cage catalyst loaded with gold nanoparticles.
[0064] Test Example 1: Catalytic Effect Test of Janus Cage Catalyst
[0065] The Janus cage catalysts prepared in Example 1 and Comparative Examples 1-3 were used for catalytic testing. The specific steps were as follows: 0.1 g of Janus cage catalyst was dispersed in 100 ml of water, 0.1 g of nitrobenzene and 0.1 g of NaBH4 were added, and the reaction was carried out at 45° C. for 10 min. The conversion rate of nitrobenzene was detected by UV-visible spectroscopy. The results are shown in Table 1 below.
[0066] Table 1 Conversion rate of nitrobenzene
[0067] Conversion rate Example 1 96.5% Comparative Example 1 15.7% Comparative Example 2 1.2% Comparative Example 3 7.8%
[0068] Nitrobenzene is reduced to aniline by sodium borohydride in the presence of Au catalyst. From the data in Table 1, it can be seen that the Janus cage catalyst prepared in Example 1 has a good catalytic effect on the reduction of nitrobenzene. Because 45°C is greater than the lower critical solution temperature (LCST) of PNIPAM, the inner surface of the shell is hydrophobic at this time, and the reactant nitrobenzene is enriched in the cavity, which is conducive to the rapid catalysis of the reaction by Au.
[0069] The only difference between Comparative Example 1 and Example 1 is that the temperature-sensitive polymer monomer N-isopropylacrylamide is not added, resulting in the prepared catalyst not having temperature responsiveness. Although Au can be complexed with azobiscyanovaleric acid, at 45°C, the inner surface is still a hydrophilic surface and cannot induce the reactant nitrobenzene to enrich inside it, resulting in Au being unable to catalyze the reduction of nitrobenzene well.
[0070] The difference between Comparative Example 2 and Example 1 is that azobisisobutyramidine hydrochloride is used as an initiator instead of azobiscyanovaleric acid. Azobisisobutyramidine hydrochloride cannot be complexed with Fe, resulting in the absence of an initiator in the entire reaction, so the temperature-sensitive polymer monomer cannot be effectively polymerized, and the final product is Fe3O4@SiO2 inorganic magnetic cage, which has no catalytic effect. Therefore, the catalytic efficiency of sodium borohydride for nitrobenzene is extremely low.
[0071] The difference between Comparative Example 3 and Example 1 is that ethyl orthosilicate is not added, so the inner and outer surfaces of the shell are both ferrosoferric oxide, and finally the inner and outer surfaces of the shell are grafted with PNIPAM, which does not have Janus characteristics. At 45°C, PNIPAM is hydrophobic, resulting in the entire catalyst not being well dispersed in water, so Au cannot effectively catalyze the reaction.
[0072] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a responsive Janus cage catalyst, characterized in that: The steps include: S1. Preparation of sulfonated polystyrene spheres: polystyrene spheres are mixed with concentrated sulfuric acid, reacted for 1-6 hours, the reaction mixture is dripped into water, filtered, washed several times until the filtrate is neutral, and vacuum dried to obtain sulfonated polystyrene spheres; Preparation of S2.PS@Fe3O4 balls: Disperse the dried sulfonated polystyrene balls in water, introduce nitrogen to remove oxygen in the system, add ferric chloride and ferrous chloride, stir for 12-24 hours, filter, disperse again in deoxygenated water, add NaOH aqueous solution, adjust the pH to 10-12, react for 1-3 hours, filter, wash several times until the filtrate is neutral, and vacuum dry to obtain PS@Fe3O4 balls; S3. Preparation of inorganic magnetic cages: PS@Fe3O4 balls were dispersed in ethanol, tetraethyl orthosilicate was added, ammonia water was added, the reaction was stirred for 3-6 hours, and centrifuged to wash to obtain PS@Fe3O4@SiO2 balls, and an organic solvent was added to remove polystyrene to obtain Fe3O4@SiO2 inorganic magnetic cages; S4. Preparation of responsive Janus cage: disperse Fe3O4@SiO2 inorganic magnetic cage in water, add initiator, stir for 1-3h, filter, disperse in water again, add monomer of thermosensitive polymer, react at 60-80℃ for 6-12h, separate by magnetic separation, wash, dry, and obtain temperature responsive Janus cage; S5. Preparation of responsive Janus cage catalyst: disperse the temperature-responsive Janus cage in water, add chloroauric acid, stir for 1-3 hours, filter, disperse in water again, add sodium borohydride, react for 1-2 hours, and obtain a responsive Janus cage catalyst loaded with gold nanoparticles.
2. The method for preparing the responsive Janus cage catalyst according to claim 1, characterized in that: In the step S1, the polystyrene balls are linear polystyrene balls, and the mass ratio of the polystyrene balls to the concentrated sulfuric acid is 1:5-20.
3. The method for preparing the responsive Janus cage catalyst according to claim 1, characterized in that: In the step S2, the molar ratio of ferric chloride to ferrous chloride is 1:1, and the mass ratio of the sulfonated polystyrene balls to ferric chloride is 1:5-20.
4. The method for preparing the responsive Janus cage catalyst according to claim 1, characterized in that: In the step S3, the mass ratio of PS@Fe3O4 balls, ethanol and tetraethyl orthosilicate is 1:20-30:4-8, the concentration of ammonia water added is 2-5wt%, and the organic solvent added is a good solvent for polystyrene.
5. The method for preparing the responsive Janus cage catalyst according to claim 4, characterized in that: In step S3, the organic solvent is selected from one of toluene, dimethylformamide, dimethylacetamide, chloroform and tetrahydrofuran.
6. The method for preparing the responsive Janus cage catalyst according to claim 1, characterized in that: In the step S4, the initiator is a carboxyl-containing initiator, which is azobiscyanovaleric acid; the mass ratio of the Fe3O4@SiO2 inorganic magnetic cage to the initiator is 1:1-3.
7. The method for preparing the responsive Janus cage catalyst according to claim 1, characterized in that: In step S4, the monomer of the thermosensitive polymer is selected from one of N-isopropyl acrylamide, N,N-diethyl acrylamide, N-(L)-(1-hydroxymethyl)propyl methacrylamide, and N-acryloyloxy-N-alkylpiperazine; the mass of the monomer of the thermosensitive polymer is 3-5 times the mass of the Fe3O4@SiO2 inorganic magnetic cage.
8. The method for preparing the responsive Janus cage catalyst according to claim 1, characterized in that: In step S5, the mass of the chloroauric acid is 0.1-1 times the mass of the temperature-responsive Janus cage, and the mass of the sodium borohydride is 0.1-0.5 times the mass of the temperature-responsive Janus cage.
9. A responsive Janus cage catalyst prepared by the preparation method according to any one of claims 1 to 8.
10. Use of a responsive Janus cage catalyst prepared by the preparation method according to any one of claims 1 to 8 in phase transfer catalysis.