Phosphorite beneficiation method
By synchronously decarbonizing and demagnesium decarbonization in the phosphate ore ore dressing process, the problem of removing carbonaceous and magnesium impurities in high-carbonaceous phosphate ore is solved, and phosphorus is improved The grade and recovery rate of concentrate simplifies the process flow and achieves efficient production of phosphorus concentrate.
Patent Information
- Application Number
- CN202411114709.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
When the existing phosphate ore ore treatment process is used to treat high carbonaceous phosphate ore, the decarbonization and demagnesium decarbonation process are complex and low efficiency, resulting in a decrease in the recovery rate of phosphorus concentrate, and the high content of carbonaceous components affects the flotation effect, resulting in production. Not high rate and taste.
By synchronous decarbonization and demagnesium removal, the process is simplified by adding decarbonization collectors and demagnesium removal collectors in the flotation process, and the synergistic effect is used to strengthen the efficient removal of carbonaceous and magnesium impurities and simplify the process flow. And improve the grade and recovery of phosphorus concentrate.
It has achieved efficient removal of carbonaceous and magnesium impurities from phosphate ores, improved the yield and recovery of phosphate concentrates, simplified the process flow, reduced the impact of carbonaceous components on flotation, and enabled the rapid settlement of phosphate concentrates. , improves the grade and recovery rate of phosphorus concentrate.
Smart Images

Figure CN119016202A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of mineral processing, and more specifically, to a method for mineral processing of phosphate ore. Background Art
[0002] Phosphorus is one of my country's strategic non-metallic mineral resources and a non-renewable resource. It has important uses in agriculture and industry. It is one of the essential elements for plant growth and is crucial to increasing crop yields and improving soil quality. It is widely used in the production of fertilizers and animal husbandry to promote agricultural production. It is also one of the important raw materials for electrode materials in the new energy industry, such as lithium iron phosphate batteries. Phosphate ore is one of the main sources of phosphorus. It is mainly found in igneous rocks, sedimentary rocks and metamorphic rock bodies. my country's proven collophanites account for about 80% of the total phosphorus resources, and mainly exist in the form of medium and low-grade collophanites. With the continuous mining and utilization of phosphate resources, the properties of the ore are gradually approaching poor, fine and mixed. In addition, the structural characteristics of collophanites themselves, such as the carbonaceous components, carbonates and other substances contained, make this type of ore more difficult to select. Therefore, improving the beneficiation level of medium and low-grade phosphate ore is of great significance for the rational development and utilization of my country's phosphate resources.
[0003] The main beneficiation processes for phosphate ore include photoelectric selection, flotation, gravity separation, magnetic separation, microbial synergistic enhancement and many combined processes. Among them, flotation is one of the most commonly used phosphate ore beneficiation methods. It mainly adjusts the interface physical and chemical properties of phosphate ore and associated gangue minerals by adding flotation agents, so as to achieve the selective flotation separation of phosphate ore and gangue minerals. The main components of medium and low-grade collophanite are P2O5, SiO2, CaO, MgO and carbonaceous substances. Among them, due to the light weight and good adsorption of carbon, it will be adsorbed on useful minerals and gangue minerals during the flotation process, which will reduce the floatability of these minerals and affect the flotation yield. In addition, carbonaceous substances also have a strong adsorption capacity for the collectors used in the flotation process, thereby affecting the mineral recovery rate; therefore, in order to achieve higher quality beneficiation of collophanite, many researchers have carried out decarbonization treatment in phosphate flotation to reduce the influence of carbonaceous substances on phosphate beneficiation.
[0004] For example, Chinese patent CN105597939A discloses a low-grade calcareous silicate colloidal phosphate beneficiation process, comprising the following steps: (A) crushing; (B) ball milling: -200 mesh accounts for 80-95%, preferably 95%, and enters the flotation decarbonization process; (C) flotation decarbonization: adding water to adjust the slurry to a mass concentration of 20-40%, adding a mixture of collector acyl ester and sodium oleate and a foaming agent pine oil to the slurry, mixing, stirring evenly and flotation decarbonization; the tailings enter the first reverse flotation sweeping selection; the product in the tank enters the direct flotation roughing selection; (D) direct flotation desiliconization roughing selection: using sodium carbonate as an adjusting agent to adjust the pH value to 9-11, while using water glass as an inhibitor, and using acyl ester and sodium oleate The mixture is subjected to forward flotation roughing; the tailings directly enter the tailings pond; the concentrate enters the reverse flotation section; (E) reverse flotation demagnesization: including reverse flotation roughing and reverse flotation scavenging. The reverse flotation roughing is to adjust the pH value to 4-6 with sulfuric acid as an adjusting agent, phosphoric acid as an inhibitor, and butter as a collector for roughing. The reverse flotation concentrate is concentrated and filtered to obtain a concentrate cake. The foam product obtained by the reverse flotation roughing enters the first stage of reverse flotation scavenging, wherein the pH value is adjusted to 3.5-3.9 with sulfuric acid. The product in the tank of the first stage of reverse flotation scavenging is the reverse flotation concentrate, which returns to the reverse flotation roughing process, a roughing and three scavenging reverse flotation; the carbon content in the phosphate ore of the invention is 12%-21%, and the carbon content after flotation is less than 3%.
[0005] For another example, Chinese patent CN103909017A discloses a flotation process for a mixed type of collophanite containing organic carbon, wherein a flotation decarbonization, a positive flotation desiliconization and a reverse flotation demagnesiumization process are used for a collophanite containing 1 to 10% of organic carbon by mass, and an anionic fatty acid collector and diethyl phthalate are used for flotation decarbonization, including adding water to the mixed type of collophanite containing organic carbon, crushing and grinding to obtain a pulp with a mass concentration of 20 to 40%, adding a collector and a frother to the pulp for mixed flotation, and the obtained foam is The product is carbon-containing tailings, and the product in the tank enters a direct flotation desiliconization process; the direct flotation desiliconization process includes adjusting the pH value to 9-11 with sodium carbonate as an adjusting agent, using water glass as an inhibitor, and using an anionic fatty acid collector for direct flotation roughing, and the obtained foam product enters a reverse flotation demagnesization process; the reverse flotation demagnesization process includes adjusting the pH value to 4-6 with sulfuric acid as an adjusting agent, using phosphoric acid as an inhibitor, and using an anionic fatty acid collector for reverse flotation roughing in a flotation machine, and the obtained product in the tank is a phosphate concentrate.
[0006] For example, Chinese patent CN115532445A discloses a flotation process for high-magnesium medium-low-grade collophanite, in which a decarbonization step of the raw ore is added before the demagnesing process, wherein the decarbonization agent is a mixture of 50-70wt% citric acid aqueous solution and diesel in a ratio of 5-15:1; during the decarbonization treatment, the raw ore is ball-milled to form a 20-30wt% ore pulp, the pH is adjusted to 4.8-5.0, the decarbonization agent is added, stirred evenly, and then aerated for reverse flotation, and the decarbonized concentrate at the bottom of the flotation tank is collected for subsequent treatment; that is, acid is first added to the decarbonized concentrate to adjust the pH 4.5~4.8, then add a demagnesium collector to carry out reverse flotation operation of demagnesium roughing, and collect the concentrate pulp at the bottom of the flotation tank; add phosphoric acid and a demagnesium collector to the concentrate pulp in sequence to carry out reverse flotation operation of demagnesium selection, and the pulp at the bottom of the flotation tank is the final concentrate; the organic carbon content in the phosphate rock of the invention is 1.63%~1.89%, and the decarbonization treatment reduces the organic carbon content in the pulp, which alleviates the adsorption effect of organic carbon on the demagnesium agent.
[0007] For another example, Chinese patent CN110369152A discloses a flotation process for fine phosphate ore, comprising the following steps: (1) Ball milling: make the mass fraction of phosphate ore with a fineness of less than 500 mesh higher than 90%; (2) Reverse flotation decarbonization and demagnesiumization: add water to adjust the pulp to a pulp concentration of 20-26%, stir and add phosphoric acid and diesel to adjust the pulp, add reverse flotation collector fatty acid soap collector XF-1 under pH 5.4-5.8 and stir evenly, aerate flotation to reduce the influence of organic carbon on flotation desiliconization and demagnesiumization, and collect the reverse flotation decarbonization and demagnesiumization concentrate in the flotation tank; (3) Direct flotation desiliconization: add sodium carbonate to adjust the decarbonization and demagnesiumization concentrate pulp, and carry out desiliconization flotation under pH 9.5-9.8; (4) Reverse flotation demagnesiumization: add phosphoric acid to adjust the desiliconization concentrate pulp, and carry out demagnesiumization flotation under pH 5.3-5.6; The invention method does not indicate the carbon content contained in the phosphate ore.
[0008] In summary, although the existing processes have taken into account the influence of carbonaceous matter in phosphate ore on phosphate ore beneficiation and thus carried out decarbonization treatment, the carbonaceous matter content in the phosphate ore is relatively low, and most of them carry out a decarbonization pretreatment process before the demagnesium and desiliconization processes. It has not taken into account the influence of high carbonaceous matter content in phosphate ore on phosphate ore beneficiation, and has also made the beneficiation process more lengthy. Summary of the invention
[0009] In view of the above, the present invention provides a phosphate ore beneficiation method, which is aimed at medium and low-grade phosphate ore with a high content of carbonaceous components, wherein the carbonaceous components include clay and other carbonaceous components with a total content of 18-46%. A decarbonization collector and a demagnesium collector are added simultaneously in the decarbonization and demagnesiumization stage of phosphate ore flotation to perform decarbonization and demagnesiumization twice, and the synergistic effect between the decarbonization collector and the demagnesium collector is utilized to enhance the efficient removal of carbonaceous components and magnesium impurity components, reduce the influence of carbonaceous components on demagnesiumization and desiliconization during flotation, avoid turbidity in the thickening tank, and make the phosphate concentrate settle quickly, thereby achieving efficient removal of gangue components in the phosphate ore and effective recovery of the phosphate concentrate.
[0010] The present invention provides a phosphate ore dressing method, comprising the following steps: (1) ball milling: ball milling the raw phosphate rock with a carbonaceous component content of 18-46% so that the proportion of particles ≤200 mesh is not less than 75%, and the slurry concentration is controlled to be 45-55% during the ball milling process to obtain the ball-milled phosphate rock W1; (2) Decarbonization and demagnesium roughing: water is added to adjust the pulp for decarbonization and demagnesium roughing of W1, the pulp concentration is controlled at 30-55%, sulfuric acid is added, and decarbonization collector and demagnesium collector are added at the same time. After stirring for a certain period of time, flotation is performed to obtain tailings X1 and phosphate rock K1; (3) Decarbonization and demagnesium scavenging: Decarbonization and demagnesium scavenging is performed on the phosphate rock product K1, sulfuric acid is added, and a decarbonization collector and a demagnesium collector are added at the same time. After stirring for a certain period of time, flotation is performed to obtain demagnesium-depleted middlings X2 and phosphate rock K2. The demagnesium-depleted middlings X2 are returned to step (2) for further decarbonization and demagnesium roughing; (4) Magnesium removal and scavenging: Magnesium removal and scavenging are performed on K2, and a magnesium removal collector is added. After stirring for a certain period of time, flotation is performed to obtain magnesium removal middlings X3 and phosphate ore K3. The magnesium removal middlings X3 are returned to step (3) for further decarbonization and magnesium removal scavenging; (5) Desiliconization roughing: Reverse flotation desiliconization operation is performed on K3, a desiliconization collector is added, and reverse flotation is performed after stirring for a certain period of time to obtain desiliconized middlings X4 and phosphate ore K4. The desiliconized middlings X4 are returned to step (4) for further demagnesium scavenging; (6) Desiliconization scavenging: Reverse flotation desiliconization scavenging operation is performed on K4, a desiliconization collector is added, and reverse flotation is performed after stirring for a certain period of time to obtain desiliconized middlings X5 and phosphate concentrate. The desiliconized middlings X4 are returned to step (5) for further desiliconization roughing; (7) The desiliconized ore product X5 is returned to step (6) for further desiliconization and scavenging; The decarbonizing collectors in steps (2) to (3) are all mixtures of diesel, pine oil and isooctyl alcohol, the demagnesiumizing collectors in steps (2) to (4) are all mixtures of oxidized paraffin soap, sodium dodecylbenzene sulfonate and sodium dodecyl sulfate, and the desiliconizing collectors in steps (5) to (6) are all mixtures of dodecylamine, tetrabutylammonium chloride and cocamidopropyl betaine.
[0011] The carbonaceous components in the original phosphate ore have an adverse effect on the flotation of phosphate ore: due to its good adsorption, it will adsorb on useful minerals and gangue minerals, reducing the floatability of these minerals and affecting the flotation yield. It also has a strong adsorption capacity for collectors, thereby increasing the amount of collectors and affecting the recovery rate of minerals. In addition, the presence of carbonaceous components, especially high-content carbonaceous components, will have many adverse effects on the flotation process of phosphate ore. For example, carbonaceous components will reduce the floatability of minerals, reduce the grade and yield of phosphate concentrates, and if the carbonaceous components cannot be effectively removed, it will cause the suspension of hydrophobic particles, which cannot be removed in the thickening tank. Ineffective sedimentation leads to turbidity of the slurry. In addition, the carbonaceous component will interfere with the flocculation process, making the flocculation effect worse, and the particles in the slurry are difficult to aggregate and settle, which leads to turbidity in the thickening tank during the flotation process. The phosphate concentrate cannot settle quickly, affecting the yield and grade of the phosphate concentrate; at the same time, the higher the content of the carbonaceous component, the more difficult it will be to remove magnesium and silicon from the flotation, because the high carbonaceous component will compete with magnesium-containing minerals and siliceous minerals for adsorption, reducing the effectiveness of the collector, resulting in poor magnesium and silicon removal effects. Therefore, it is necessary to effectively remove the carbonaceous component in the phosphate ore and improve the efficiency of flotation magnesium removal and silicon removal, thereby improving the grade and recovery rate of the phosphate concentrate.
[0012] The present invention proposes that the phosphate ore with high carbon content be demagnesized and decarburized simultaneously. Compared with the two-step process of first decarburizing and then demagnesizing, the method of the present invention for demagnesizing and decarburizing simultaneously is more efficient and simple: because for the phosphate ore with high carbon content, if the process of first decarburizing and then demagnesizing is adopted, not only the process is complicated, but also more phosphorus component entrainment loss will be caused, resulting in a decrease in the recovery rate of the phosphate concentrate; therefore, the present invention proposes that when the content of carbonaceous components in the phosphate ore is high, a process of simultaneously pre-disposing the carbonaceous components and the magnesium impurity components is adopted, and the synergistic effect between the collectors for decarburization and demagnesizing is utilized. The effect is to strengthen the efficient removal of carbon and magnesium impurity components, which not only ensures that the magnesium content in the obtained phosphate concentrate is within the qualified range, but also makes the impurity components in the phosphate ore that mainly affect the phosphate concentrate the siliceous components after the phosphate ore is decarbonized and demagnesized. Finally, a desiliconization collector and a "one rough and one sweep" phosphate ore flotation desiliconization process are used to achieve the effective removal of the siliceous components in the phosphate ore, and the intermediate ore products of each step are returned in sequence for re-floatation to form a process closed loop. In this way, the removal of impurity components such as carbon, magnesium, and silicon in the phosphate ore can be more effectively achieved, and the yield and recovery rate of the phosphate concentrate can be improved.
[0013] The pulp concentration is controlled at 30-55% during the flotation process. The appropriate pulp concentration can make the ore particles flow freely with the liquid and effectively contact with the collector and other reagents, so that the flotation is more sufficient; at the same time, the present invention adopts the simultaneous addition of the decarbonization collector and the demagnesium collector, wherein the decarbonization collector is mainly a nonionic surfactant, and the demagnesium collector is mainly an anionic surfactant. The simultaneous addition of nonionic and anionic surfactants can enhance the interfacial activity, so that the carbonaceous impurities and magnesium-containing minerals in the pulp form a stable attachment system with the bubbles at the same time. The synergistic effect of the two can improve the flotation selectivity, and can better achieve the effective removal of the carbonaceous components and magnesium impurity components in the phosphate ore. Simultaneous decarbonization and demagnesium can simplify the use of reagents and the regulation of pulp conditions, and improve the economy and operating efficiency of the process. In addition, magnesium-containing minerals and carbonaceous impurities have more similar physical and chemical properties in the flotation process, and the flotation behavior of siliceous impurities is quite different, so they are more suitable for simultaneous decarbonization and demagnesium treatment.
[0014] The P2O5 content of the original phosphate rock is 17-25%, the MgO content is 4-7%, and the SiO2 content is 11-33%.
[0015] The magnesium impurity component in the original phosphate ore is mainly magnesium oxide, and the silicon impurity component is mainly silicon dioxide.
[0016] The sulfuric acid added in the decarbonization and demagnesium roughing of step (2) is 30-45 kg / t of original phosphate ore, and the sulfuric acid added in the decarbonization and demagnesium scavenging of step (3) is 5-10 kg / t of original phosphate ore. Sulfuric acid is an acidic adjusting agent, and the appropriate amount of acid is used to adjust the pulp concentration to achieve the pH index of flotation and help improve the adhesion or contamination layer on the surface of the ore particles, so as to improve the flotation-related properties of the surface of the ore particles.
[0017] The amount of the decarbonization collector added in the decarbonization and demagnesium roughing of step (2) is 200-350 g / t of original phosphate ore, and the amount of the demagnesium collector added is 700-800 g / t of original phosphate ore; the amount of the decarbonization collector added in the decarbonization and demagnesium sweeping of step (3) is 50-90 g / t of original phosphate ore, and the amount of the demagnesium collector added is 150-200 g / t of original phosphate ore.
[0018] The decarbonization collector is a mixture of diesel, pine oil and isooctyl alcohol in a mass ratio of 2-4:1-2.5:0.5-1. The appropriate ratio of the three substances has higher surface activity, so that the carbonaceous components in the phosphate rock can be efficiently removed; the magnesium removal collector is a mixture of oxidized paraffin soap, sodium dodecylbenzene sulfonate and sodium dodecyl sulfate in a mass ratio of 3-4:2-3:1.5-2. Similarly, the appropriate ratio of the three substances has higher surface activity, which enhances the effective removal of magnesium oxide.
[0019] The dosage of decarbonization collector and demagnesium collector is closely related to the content of carbonaceous components and magnesium oxide in phosphate ore. When the content of carbonaceous components and magnesium oxide in phosphate ore is high, the dosage of decarbonization collector and demagnesium collector should be increased. However, if the dosage of corresponding collector is too much, it may cause the foam layer to be unstable, the target mineral cannot be captured by the foam or the foam layer breaks and loses the capture effect of the target mineral, so that the quality of phosphate concentrate is reduced. If the dosage of corresponding collector is too little, the target mineral may not be fully aggregated into the foam layer, resulting in reduced flotation efficiency. At the same time, The appropriate amount of decarbonization collector and demagnesium collector can better exert their synergistic effect and improve the removal efficiency; at the same time, the carbonaceous components and magnesium oxide in the original phosphate ore have been mostly removed after the decarbonization and demagnesium roughing in step (2), and the decarbonization and demagnesium scavenging in step (3) is to further remove the residual carbonaceous components and magnesium oxide in the ore pulp; and the carbonaceous components in the phosphate ore are fully utilized in the decarbonization and demagnesium flotation in steps (2) and (3) through the reasonable use of collectors, so that the synergistic effect between different collectors is fully exerted, so that the decarbonization collector is fully dispersed in the ore pulp and covers the The surface of the carbonaceous component, these decarbonizing collectors combine with the carbonaceous component to form a hydrophobic film on its surface, forming a carbonaceous component-collector complex, making the surface of the carbonaceous component more hydrophobic, so that it is easier to combine with bubbles, and then through flotation separation, the purpose of removing the carbonaceous component is achieved; similarly, the magnesium removal collector combines with magnesium oxide to form a hydrophobic film on its surface, forming a magnesium oxide-collector complex, making the surface of magnesium oxide more hydrophobic, so that it is easier to combine with bubbles, and then through flotation separation, the purpose of removing magnesium oxide is achieved; and in this process Because of the synergistic effect of the decarbonization collector and the demagnesiumization collector, the interfacial activity of the two collectors is improved, and they can better combine with the carbonaceous components and magnesium oxide to form a more stable complex, so that the removal of the carbonaceous components and magnesium oxide is more thorough; therefore, for the phosphate ore with high carbon content in the present invention, using 200-350g / t of decarbonization collector and 700-800g / t of demagnesiumization collector and 50-90g / t of decarbonization collector and 150-200g / t of demagnesiumization collector for two decarbonization and demagnesiumization flotation can obtain a more ideal flotation index.
[0020] The amount of the magnesium removal collector added in the magnesium removal scavenging in step (4) is 50 g / t of original phosphate rock. Most of the magnesium oxide in the slurry has been removed in the decarbonization and magnesium removal flotation in steps (2) and (3). The magnesium removal scavenging is performed again to remove the magnesium oxide in the slurry as much as possible, so that the magnesium oxide content in the final phosphate concentrate is lower.
[0021] The mass ratio of dodecylamine, tetrabutylammonium chloride and cocamidopropyl betaine is 1.5-2.5:0.5-1:0.5-1. Similarly, the three substances with appropriate proportions can exert the synergistic effect between the components, make their surface activity higher, strengthen the flotation separation of silicon dioxide in the ore pulp, and reduce the silicon dioxide content in the phosphate concentrate.
[0022] The amount of the desiliconization collector added in the desiliconization rough selection in step (5) is 300-600 g / t of the original phosphate rock, and the amount of the desiliconization collector added in the desiliconization sweep selection in step (6) is 100-250 g / t of the original phosphate rock.
[0023] The dosage of the desiliconization collector mainly depends on the content of silicon dioxide in the original phosphate ore. When the content of silicon dioxide in the original phosphate ore is high, the dosage of the desiliconization collector used in step (5) desiliconization roughing must be increased so that the silicon component in the phosphate ore can be better removed, thereby obtaining a phosphate concentrate with a low silicon dioxide content; wherein step (5) desiliconization roughing can achieve the removal of most of the silicon components in the phosphate ore, and step (6) performs a desiliconization sweeping operation again, which can further remove the silicon dioxide in the phosphate ore, and finally obtain a phosphate concentrate with a low silicon dioxide content.
[0024] The stirring rate in steps (2) to (6) is 1600 to 1900 r / min, the stirring time is 3 to 5 min, and the flotation time is 3 to 6 min.
[0025] The appropriate stirring rate can provide a suitable fluid dynamic environment for pulp flotation, which can ensure the dispersion and flotation separation between mineral particles, and stir for a certain time to allow the reagent to fully act on the pulp system and the mineral particles to fully act on the flotation reagent, thereby ensuring a good sorting effect. At the same time, the appropriate flotation time ensures that the target mineral can be fully floated and separated from the pulp system. If the time is too short, the foam product cannot be effectively separated, and if the time is too long, unnecessary energy consumption will be caused.
[0026] The P2O5 content of the phosphate concentrate is 30.76-34.26%, the MgO content is 0.94-1.08%, and the SiO2 content is 6.27-6.93%.
[0027] In summary, the present invention proposes a method for improving the beneficiation index of phosphate ore with a carbonaceous component content of 18-46%, and effectively removes the carbonaceous component and the magnesium impurity component in the slurry by performing two decarbonization and demagnesium removal. At the same time, the present invention simultaneously adds a decarbonization collector and a demagnesium collector to perform decarbonization and demagnesium removal. The process is not only simple, but also utilizes the synergistic effect between the decarbonization collector and the demagnesium collector, so that the surface activity of the collector is better, and the adsorption of the carbonaceous component and the magnesium impurity component is more effective, and finally the high-content carbonaceous component in the phosphate ore is effectively removed and most of the magnesium impurity components are removed, which greatly reduces the carbonaceous component on the phosphate ore. The effect of flotation can make the phosphate concentrate settle quickly, obtain qualified phosphate concentrate and its effective recovery; and through the flotation process of "one rough and one sweep" decarbonization and magnesium removal followed by magnesium removal and scavenging again, as well as "one rough and one sweep" desiliconization and "sequential return of medium ore", the beneficiation enrichment and process closure of medium and low grade phosphate ore with high carbonaceous content are realized, and the efficient removal of gangue components such as magnesium oxide and silicon dioxide in the phosphate ore is achieved, so that the P2O5 content in the final phosphate concentrate is 30.76-34.26%, the MgO content is 0.94-1.08%, the SiO2 content is 6.27-6.93%, and the recovery rate of P2O5 is above 70%. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a process flow chart of phosphate ore dressing. DETAILED DESCRIPTION
[0029] The embodiments of the present application will be described in more detail below. The application can be implemented in various forms, and should not be construed as being limited to the embodiments set forth herein, but rather these embodiments are provided to provide a more thorough and complete understanding of the present application. It should be understood that the embodiments of the present application are only for exemplary purposes and are not intended to limit the scope of protection of the present application.
[0030] The process flow of phosphate ore dressing of the present invention is as shown in the attached figure. Figure 1 As shown, the embodiment is implemented according to the following technical solution: (1) ball milling: ball milling the raw phosphate rock with a carbonaceous component content of 18-46%, controlling the slurry concentration to 45-55% during the ball milling process, and making the -200 mesh content not less than 75%, to obtain the ball-milled phosphate rock W1; (2) Decarbonization and demagnesium roughing: water is added to adjust the pulp for decarbonization and demagnesium roughing of W1, the pulp concentration is controlled at 30-55%, 30-45 kg / t of sulfuric acid of the original phosphate ore is added, and 200-350 g / t of the original phosphate ore decarbonization collector and 700-800 g / t of the original phosphate ore demagnesium collector are added at the same time. After stirring at a stirring rate of 1600-1900 r / min for 3-5 min, flotation is performed for 3-6 min to obtain tailings X1 and phosphate ore K1; (3) Decarbonization and demagnesium separation: Decarbonization and demagnesium separation is performed on the phosphate ore product K1. 5-10 kg / t of sulfuric acid is added to the original phosphate ore. 50-90 g / t of decarbonization collector and 150-200 g / t of demagnesium collector are added to the original phosphate ore. After stirring for 3-5 min at a stirring rate of 1600-1900 r / min, flotation is performed for 3-6 min to obtain demagnesium-free middlings X2 and phosphate ore K2. The demagnesium-free middlings X2 are returned to step (2) for decarbonization and demagnesium-free roughing. (4) Magnesium removal scavenging: Magnesium removal scavenging operation is performed on K2, and 50 g / t of magnesium removal collector of original phosphate ore is added. After stirring for 3 to 5 minutes at a stirring rate of 1600 to 1900 r / min, flotation is performed for 3 to 6 minutes to obtain magnesium removal middlings X3 and phosphate ore K3. The magnesium removal middlings X3 are returned to step (3) for further decarbonization and magnesium removal scavenging; (5) Desiliconization roughing: Reverse flotation desiliconization operation is performed on K3, and 300-600 g / t of desiliconization collector of original phosphate ore is added. After stirring for 3-5 min at a stirring rate of 1600-1900 r / min, flotation is performed for 3-6 min to obtain desiliconized middlings X4 and phosphate ore K4. The demagnesized middlings X4 are returned to step (4) for demagnesized scavenging; (6) Desiliconization scavenging: Reverse flotation desiliconization scavenging operation is performed on K4, 100-250 g / t of desiliconization collector of original phosphate ore is added, stirring at a stirring rate of 1600-1900 r / min for 3-5 min, and then flotation is performed for 3-6 min to obtain desiliconized middlings X5 and phosphate concentrate, and the desiliconized middlings X4 are returned to step (5) for further desiliconization roughing; (7) The desiliconized ore product X5 is returned to step (6) for further desiliconization and scavenging; The decarbonizing collectors used in the above steps are all mixtures of diesel, pine oil and isooctyl alcohol in a mass ratio of 2-4:1-2.5:0.5-1; the demagnesium collectors used are all mixtures of oxidized paraffin soap, sodium dodecylbenzene sulfonate and sodium dodecyl sulfate in a mass ratio of 3-4:2-3:1.5-2; and the desiliconizing collectors used are all mixtures of dodecylamine, tetrabutylammonium chloride and cocamidopropyl betaine in a mass ratio of 1.5-2.5:0.5-1:0.5-1.
[0031] The specific process conditions of the embodiment are shown in Table 1, wherein the pulp concentration will change with the process from the initial decarbonization and demagnesium roughing to the final desiliconization scavenging. Similarly, the stirring rate will be adjusted according to the change of the pulp concentration. Therefore, for each group of experiments, the pulp mass concentration is controlled at 30-55% and the stirring rate is controlled at 1600-1900r / min during the flotation process.
[0032] Comparative Example: Using the original phosphate rock used in Example 3 as raw material, a phosphate rock beneficiation process of single decarburization, followed by demagnesiumization and desiliconization was adopted, and the specific steps were as follows: (1) Ball milling: The original phosphate rock with a carbonaceous component content of 46% is ball milled, and the slurry concentration is controlled to be 55% during the ball milling process, so that the -200 mesh content is not less than 75%, and the ball-milled phosphate rock W1 is obtained; (2) Decarbonization roughing: water was added to adjust the pulp for flotation decarbonization of W1, the pulp concentration was controlled at 30%, 45 kg / t of sulfuric acid of the original phosphate rock was added, and 350 g / t of the original phosphate rock decarbonization collector was added at the same time. After stirring at a stirring rate of 1600 r / min for 5 min, flotation was performed for 6 min to obtain tailings W2 and phosphate rock W3; (3) Decarbonization scavenging: Decarbonization scavenging is performed on the phosphate ore product W3 by adding 10 kg / t of sulfuric acid of the original phosphate ore and 90 g / t of the original phosphate ore as a decarbonization collector. After stirring at a stirring rate of 1600 r / min for 5 min, flotation is performed for 6 min to obtain decarbonized middlings W4 and phosphate ore W5. The decarbonized middlings W4 are returned to step (2) for further decarbonization roughing. (4) Magnesium removal roughing: The phosphate ore product W5 was subjected to magnesium removal roughing, and 700 g / t of magnesium removal collector of the original phosphate ore was added. After stirring for 5 min at a stirring rate of 1600 r / min, flotation was performed for 6 min to obtain magnesium removal middling ore X1 and phosphate ore K1; (5) Magnesium removal scavenging: The phosphate ore product K1 is subjected to magnesium removal scavenging, and 150 g / t of magnesium removal collector of the original phosphate ore is added, and after stirring at a stirring rate of 1600 r / min for 5 min, flotation is performed for 6 min to obtain magnesium removal middlings X2 and phosphate ore K2. The magnesium removal middlings X2 are returned to step (4) for magnesium removal roughing; (6) Magnesium removal scavenging: Magnesium removal scavenging is performed on K2, and 50 g / t of the original phosphate rock is added with a magnesium removal collector. After stirring for 5 min at a stirring rate of 1600 r / min, flotation is performed for 6 min to obtain magnesium removal middlings X3 and phosphate rock K3. The magnesium removal middlings X3 are returned to step (5) for further magnesium removal scavenging; (7) Desiliconization roughing: Reverse flotation desiliconization operation is performed on K3, and 600 g / t of desiliconization collector of original phosphate ore is added. After stirring for 5 min at a stirring rate of 1600 r / min, flotation is performed for 6 min to obtain desiliconized middlings X4 and phosphate ore K4. The demagnesized middlings X4 are returned to step (6) for demagnesized scavenging; (8) Desiliconization scavenging: Reverse flotation desiliconization scavenging operation is performed on K4, 250 g / t of desiliconization collector of original phosphate ore is added, stirring at a stirring rate of 1600 r / min for 5 min, and then flotation is performed for 6 min to obtain desiliconized middlings X5 and phosphate concentrate. The desiliconized middlings X4 are returned to step (7) for further desiliconization roughing; (9) The desiliconized ore product X5 is returned to step (8) for further desiliconization scavenging; The decarbonization collectors used in the specific steps of the comparative example are all mixtures of diesel, pine oil and isooctyl alcohol in a mass ratio of 4:2.5:1, the demagnesium collectors used are all mixtures of oxidized paraffin soap, sodium dodecylbenzene sulfonate and sodium dodecyl sulfate in a mass ratio of 4:3:2, and the desiliconization collectors used are all mixtures of dodecylamine, tetrabutylammonium chloride and cocamidopropyl betaine in a mass ratio of 2.5:1:1.
[0033] Table 1 shows the specific implementation conditions of the embodiment of the present invention, Table 2 shows the contents of each component of the original phosphate ore and phosphate concentrate of the embodiment, and Table 3 shows the yield, P2O5 grade and P2O5 recovery rate of each product of the embodiment. It is proved by the experiment that the low-grade phosphate ore with high carbon content can be effectively removed by flotation through the ore dressing method of the present invention, the carbonaceous components can be effectively increased, the content of P2O5 can be effectively increased, the content of MgO and SiO2 can be reduced, the grade of the phosphate ore can be increased and the phosphate concentrate can be effectively recovered.
[0034] It can be seen from Tables 2 and 3 that the P2O5 grade of the phosphate ore obtained by the phosphate ore dressing method of the present invention is significantly improved, from 17.56-24.28% to 30.76-34.25%, with a maximum increase of 75.17%. At the same time, the recovery rate of P2O5 is above 70%, the MgO content is reduced from 4.2-6.84% to 0.94-1.08%, and the SiO2 content is reduced from 11.49-32.46% to 6.27-6.93%. Experiments have shown that the method of the present invention can effectively remove carbonaceous matter, magnesium impurities and silicon impurity components in the phosphate ore, effectively reduce the contents of magnesium oxide and silicon oxide in the phosphate ore, effectively improve the P2O5 grade of the phosphate ore and have a higher P2O5 recovery rate.
[0035] It can be seen from the comparative example that when the process of decarbonization and then demagnesium and desiliconization is used to select phosphate ore, for the same ore sample, that is, the original phosphate ore used in Example 3, the yield of phosphate concentrate is reduced from 40.21% to 37.51%, the grade is reduced from 30.76% to 29.45%, and the recovery rate is reduced from 70.44% to 62.91%, which shows that the process of the comparative example cannot efficiently obtain qualified phosphate concentrate; through the analysis of the results of Example 3 and the comparative example, it can be seen that the process of simultaneous decarbonization and demagnesiumization can give full play to the synergistic effect between the non-ionic surfactant, i.e., the decarbonization collector and the anionic surfactant, i.e., the demagnesium collector, so that the carbonaceous impurities and magnesium-containing minerals in the slurry form a stable attachment system with the bubbles at the same time, thereby improving the selectivity of flotation, thereby better realizing the effective removal of carbonaceous components and magnesium impurity components in the phosphate ore, and the simultaneous decarbonization and demagnesiumization can simplify the use of reagents and the regulation of slurry conditions, thereby improving the economy and operating efficiency of the process.
[0036] Table 1: Specific implementation conditions of the examples.
[0037] Table 2: Content of each component in the raw phosphate ore and phosphate concentrate of the examples.
[0038] Table 3: Yield, P2O5 grade and P2O5 recovery rate of each product in the example.
[0039] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in this application, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for beneficiating phosphate ore, characterized in that: The following steps are involved: (1) ball milling: ball milling the original phosphate rock with a carbonaceous component content of 18-46% so that the proportion of particles ≤200 mesh is not less than 75%, and the slurry concentration is controlled to be 45-55% during the ball milling process to obtain the ball-milled phosphate rock W1; (2) Decarbonization and demagnesium roughing: water is added to adjust the pulp concentration to 30-55%, and decarbonization and demagnesium roughing of W1 is carried out. Sulfuric acid is added, and decarbonization collector and demagnesium collector are added at the same time. After stirring for a certain period of time, flotation is carried out to obtain tailings X1 and phosphate rock K1; (3) Decarbonization and demagnesium scavenging: Decarbonization and demagnesium scavenging is performed on the phosphate rock product K1, sulfuric acid is added, and a decarbonization collector and a demagnesium collector are added at the same time. After stirring for a certain period of time, flotation is performed to obtain demagnesium-depleted middlings X2 and phosphate rock K2. The demagnesium-depleted middlings X2 are returned to step (2) for further decarbonization and demagnesium roughing; (4) Magnesium removal and scavenging: A second round of magnesium removal and scavenging operation is performed on K2, a magnesium removal collector is added, and flotation is performed after stirring for a certain period of time to obtain magnesium removal middlings X3 and phosphate ore K3. The magnesium removal middlings X3 are returned to step (3) for further decarbonization and magnesium removal scavenging; (5) Desiliconization roughing: Reverse flotation desiliconization operation is performed on K3, a desiliconization collector is added, and reverse flotation is performed after stirring for a certain period of time to obtain desiliconized middlings X4 and phosphate ore K4. The desiliconized middlings X4 are returned to step (4) for further demagnesium scavenging; (6) Desiliconization scavenging: Reverse flotation desiliconization scavenging operation is performed on K4, a desiliconization collector is added, and reverse flotation is performed after stirring for a certain period of time to obtain desiliconized middlings X5 and phosphate concentrate. The desiliconized middlings X4 are returned to step (5) for further desiliconization roughing; (7) The desiliconized ore product X5 is returned to step (6) for further desiliconization and scavenging; The decarbonizing collectors described in steps (2) to (3) are all mixtures of diesel, pine oil and isooctyl alcohol, the demagnesiumizing collectors described in steps (2) to (4) are all mixtures of oxidized paraffin soap, sodium dodecylbenzene sulfonate and sodium dodecyl sulfate, and the desiliconizing collectors described in steps (5) to (6) are all mixtures of dodecylamine, tetrabutylammonium chloride and cocamidopropyl betaine.
2. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The original phosphate rock has a P2O5 content of 17-25%, a MgO content of 4-7%, and a SiO2 content of 11-33%.
3. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The sulfuric acid in step (2) is added in an amount of 30-45 kg / t of original phosphate rock.
4. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The mass ratio of the diesel, pine oil and isooctyl alcohol is 2-4:1-2.5:0.5-1.
5. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The amount of the decarbonization collector added in step (2) is 200-350 g / t of original phosphate rock.
6. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The mass ratio of the oxidized paraffin soap, sodium dodecylbenzene sulfonate and sodium dodecyl sulfate is 3-4:2-3:1.5-2.
7. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The amount of the magnesium removal collector added in step (2) is 700-800 g / t of original phosphate rock.
8. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The amount of sulfuric acid added in step (3) is 5-10 kg / t of original phosphate rock.
9. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The amount of the decarbonization collector added in step (3) is 50 to 90 g / t of original phosphate rock.
10. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The amount of the magnesium removal collector added in step (3) is 150-200 g / t of original phosphate rock.
11. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The amount of the magnesium removal collector added in step (4) is 50 g / t of original phosphate rock.
12. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The mass ratio of the dodecylamine, tetrabutylammonium chloride and cocamidopropyl betaine is 1.5-2.5:0.5-1:0.5-1.
13. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The amount of the desiliconizing collector added in step (5) is 300-600 g / t of raw phosphate rock.
14. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The amount of the desiliconizing collector added in step (6) is 100 to 250 g / t of raw phosphate rock.
15. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The stirring rate in steps (2) to (6) is 1600 to 1900 r / min, the stirring time is 3 to 5 min, and the flotation time is 3 to 6 min.
16. A method for improving phosphate ore dressing index according to claim 1, characterized in that: The P2O5 content of the phosphate concentrate is 30.76-34.26%, the SiO2 content is 6.27-6.93%, and the MgO content is 0.94-1.08%.
Citation Information
Patent Citations
Flotation process for silicon-calcium mixed collophanite containing organic carbon
CN103909017A
Process for mineral processing of low-grade silicon calcium collophanite
CN105597939A
Micro-fine-grained phosphate ore flotation process
CN110369152A
Flotation process of high-magnesium medium-low-grade collophanite
CN115532445A
Double-reverse flotation process for silico-calcareous collophanite
CN112058503A