Semiconductor sand blasting post-cleaning system and process

By simplifying the semiconductor post-blasting cleaning system, using the combination of pre-cleaning, mortar removal and cleaning parts, the problems of high cost and large land occupation of traditional cleaning processes are solved, and efficient removal of impurities on the surface of silicon wafers is achieved, reducing equipment costs and Surrounded by area.

CN119016415APending Publication Date: 2024-11-26TIANJIN ZHONGHUAN ADVANCED MATERIAL TECH +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411339338.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The traditional semiconductor post-sandblasting cleaning process adopts 12 cleaning processes, with a total of 12 tanks, resulting in high equipment manufacturing costs, large operating costs and large area.

Method used

A semiconductor post-blasting cleaning system is designed, including a pre-cleaning part, a mortar removal part and a cleaning part. Through the optimized cleaner and ultrasonic structure, the cleaning steps are simplified, the number of tanks is reduced, and the overflow tanks and bubbles are used. Technology such as pipes improves cleaning efficiency.

Benefits of technology

The mortar and metal ions removal on the surface of semiconductor silicon wafers is achieved, which reduces the manufacturing and operating costs of the equipment, reduces the floor area, and improves the cleaning yield, so that the products meet production needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016415A_ABST
    Figure CN119016415A_ABST
Patent Text Reader

Abstract

The invention provides a cleaning system and process for a semiconductor after sand blasting, and relates to the technical field of semiconductor cleaning, the system comprises a pre-cleaning part, a mortar removing part and a cleaning part which are sequentially arranged, the pre-cleaning part is used for cleaning sand grains on the surface of a silicon wafer and comprises a first groove body, and bubbling pipes are arranged in the first groove body; the mortar removing part is used for removing mortar on the surface of the silicon wafer and comprises a second groove body, and a first cleaning agent is arranged in the second groove body; the cleaning part is used for removing particles and metal ions on the surface of the silicon wafer and comprises a third groove body, a fourth groove body and a fifth groove body which are sequentially arranged, a throwing bracket and an ultrasonic structure are arranged in the fourth groove body, a second cleaning agent is arranged in the fourth groove body, and the third groove body and the fifth groove body are each provided with a spraying pipe and a bubbling pipe. And the occupied area of the cleaning equipment is reduced. According to the technology, the system is adopted, pre-cleaning, mortar removing and surface particle and metal ion removing are included, and the cleaning yield is greatly increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor cleaning, and in particular to a semiconductor post-sandblasting cleaning system and process. Background Art

[0002] Single crystal silicon wafers are important substrate materials in the integrated circuit manufacturing process. The surface quality of polished wafers has a very important influence on the device performance of integrated circuits, such as silicon wafer surface flatness, particles, roughness, metal impurities, product appearance, etc.

[0003] The preparation of silicon materials includes directional cutting, grinding, chemical etching, sandblasting, back sealing, polishing, etc. Sandblasting is a process of spraying a certain concentration of mortar onto the surface of the silicon wafer using a wet sandblasting device with compressed air at a certain pressure to create a damaged layer, and then forming oxidation-induced stacking faults during the subsequent high-temperature heat treatment process of the back sealing process to achieve the purpose of silicon wafer external impurities. After sandblasting, mortar and other particulate impurities will remain on the surface of the silicon wafer, and the metal ions of the sandblasted product will also exceed the standard, so a post-sandblasting cleaning process is required after the sandblasting process.

[0004] The traditional sandblasting cleaning process uses multiple tanks for cleaning, and the cleaning steps are:

[0005] S1, pure water tank cleaning; S2, detergent tank cleaning; S3, detergent tank cleaning; S4, pure water tank cleaning; S5, pure water tank cleaning; S6, SC1 tank cleaning; S7, pure water tank cleaning; S8, pure water tank cleaning; S9, SC2 tank cleaning; S10, pure water tank cleaning; S11, spin drying; S12, downloading. There are 12 cleaning processes in total, and a total of 12 tanks complete the cleaning operation. The equipment manufacturing cost and operating cost are very high, and the overall equipment occupies a large area. Summary of the invention

[0006] The purpose of the present invention is to provide a semiconductor post-sandblasting cleaning system and process to solve the technical problems in the prior art that the traditional sandblasting cleaning process uses 12 cleaning processes, a total of 12 tanks to complete the cleaning operation, the equipment manufacturing cost and operating cost are very high, and the overall equipment occupies a large area. The many technical effects that can be produced by the preferred technical solution among the many technical solutions provided by the present invention are described in detail below.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] The present invention provides a semiconductor post-sandblasting cleaning system, comprising a pre-cleaning part, a slurry removal part and a cleaning part arranged in sequence, wherein:

[0009] The pre-cleaning part is used to clean sand particles on the surface of the silicon wafer, and includes a first tank body, and a bubbling tube is arranged in each of the first tank bodies;

[0010] The mortar removal part is used to remove the mortar on the surface of the silicon wafer, and includes a second tank body, in which a first cleaning agent is arranged;

[0011] The cleaning part is used to remove surface particles and metal ions from the silicon wafer, and includes a third trough body, a fourth trough body and a fifth trough body arranged in sequence, wherein a second throwing bracket and a second ultrasonic structure are arranged in the fourth trough body, and a second cleaning agent is arranged in the fourth trough body, and the third trough body and the fifth trough body are both provided with a spray pipe and a bubbling pipe.

[0012] Preferably, a first tossing bracket, a bubbling tube and a first ultrasonic structure are arranged in the second trough body, wherein the first tossing bracket is used to shake the silicon wafer; the bubbling tube is connected to a nitrogen source for bubbling; and the first ultrasonic structure is used to vibrate the silicon wafer.

[0013] Preferably, the first tank body, the third tank body and the fifth tank body are all overflow tanks.

[0014] Preferably, the first cleaning agent comprises a high-purity HF solution, and the ratio of HF to water is 1:15.

[0015] Preferably, the second cleaning agent comprises a mixed solution of deionized water, ammonia water and hydrogen peroxide, wherein:

[0016] The concentrations of ammonia solution and hydrogen peroxide solution are both 27%-32%;

[0017] The volume ratio of ammonia water: hydrogen peroxide: deionized water is 1:1:8.

[0018] Preferably, it further comprises a spin drying section, the spin drying section comprises at least one spin dryer, and the spin drying section is arranged after the cleaning section.

[0019] A semiconductor post-sandblasting cleaning process, using the semiconductor post-sandblasting cleaning system, comprises the following steps:

[0020] S1: Pre-cleaning, used to clean sand particles on the surface of silicon wafer;

[0021] S2: removing mortar, using the first cleaning agent to remove the mortar on the surface of the silicon wafer;

[0022] S3: Surface particle and metal ion removal, including:

[0023] S31: cleaning the first cleaning agent on the silicon wafer;

[0024] S32: using the second cleaning agent to remove particles and metal ions on the surface of the silicon wafer;

[0025] S33: Cleaning the second cleaning agent on the silicon wafer using the same process as step S31.

[0026] Preferably, step S31: cleaning the first cleaning agent on the silicon wafer comprises:

[0027] Dissolving the first cleaning agent on the surface of the silicon wafer, including: injecting water into the third tank and starting bubbling for a time of not less than 10 seconds;

[0028] draining the water containing the first cleaning agent in the third tank, including spraying and draining, for a period of not less than 20 seconds;

[0029] Re-injecting pure water into the third tank body for a period of not less than 70 seconds;

[0030] The above steps are repeated in sequence, water is injected and bubbling is performed to continue cleaning the silicon wafer, and the overall working time of step S31 is no more than 250 seconds.

[0031] Preferably, step S1: pre-cleaning, step S2: slurry removal, step S31: cleaning the first cleaning agent on the silicon wafer, and step S33: cleaning the second cleaning agent on the silicon wafer all include bubbling, wherein:

[0032] The bubbling nitrogen flow rate is 150L / min-180L / min; the pressure is 0.3MPa, and the diameter of the bubbling tube hole is 0.5mm.

[0033] Preferably, step S32: using the second cleaning agent to remove particles and metal ions on the surface of the silicon wafer comprises:

[0034] Use 130KHz ultrasound and clean at 55℃-65℃ for no less than 270s;

[0035] The silicon wafer is polished while being cleaned, with a polishing cycle of 20 times / min.

[0036] The semiconductor post-sandblasting cleaning system provided by the present invention comprises a pre-cleaning part, a mortar removal part and a cleaning part which are sequentially arranged, wherein the pre-cleaning part is provided with a first trough body, and the effect of removing most of the mortar attached to the surface of the semiconductor silicon wafer is achieved by combining nitrogen bubbling and pure water overflow; the mortar removal part is provided with a second trough body, and the second trough body adopts a first detergent, and the mortar on the surface of the semiconductor silicon wafer is removed by optimizing the detergent; the cleaning part comprises a third trough body, a fourth trough body and a fifth trough body, and through the cooperation of the third trough body, the fourth trough body and the fifth trough body, firstly, the first detergent on the silicon wafer is removed by the third trough body, and then, by optimizing the detergent in the fourth trough body, the second detergent is adopted to remove the particles and metal ions on the surface of the semiconductor silicon wafer, and finally, the second detergent on the silicon wafer is removed by the fifth trough body by adopting the same process as removing the first detergent on the silicon wafer. The overall structure is simple, and the mortar and particles on the surface of the silicon wafer are removed by chemical means by optimizing the liquid medicine, so as to achieve the effect of impurities on the surface of the glass silicon wafer, and the trough body is greatly simplified compared with the prior art, and the floor space occupied by the semiconductor post-sandblasting cleaning is reduced, and the equipment manufacturing cost and operation cost are effectively reduced.

[0037] The semiconductor post-sandblasting cleaning process provided by the present invention adopts the above-mentioned cleaning system, including pre-cleaning for cleaning sand particles on the surface of the silicon wafer; mortar removal, using a first cleaning agent to remove mortar on the surface of the semiconductor silicon wafer; surface particle and metal ion removal, including: cleaning the first cleaning agent on the silicon wafer; using a second cleaning agent to remove particles and metal ions on the surface of the semiconductor silicon wafer; using the same process as the first cleaning agent on the silicon wafer to clean the second cleaning agent on the silicon wafer. This semiconductor post-sandblasting cleaning process can achieve a product post-sandblasting cleaning yield of more than 99%, and the product metal and surface meet production requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 It is a structural schematic diagram of an embodiment of a semiconductor sandblasting cleaning system of the present invention;

[0040] Figure 2 It is a schematic structural diagram of the first tank body in the semiconductor post-sandblasting cleaning system of the present invention;

[0041] Figure 3 It is a schematic structural diagram of the second tank body in the semiconductor post-sandblasting cleaning system of the present invention;

[0042] Figure 4It is a schematic diagram of the structure of the third tank in the semiconductor post-sandblasting cleaning system of the present invention;

[0043] Figure 5 It is a schematic structural diagram of the fourth tank body in the semiconductor post-sandblasting cleaning system of the present invention;

[0044] Figure 6 It is a process flow chart of the semiconductor post-sandblasting cleaning process of the present invention;

[0045] Figure 7 The semiconductor sandblasting post-cleaning process of the present invention is used to produce for one week and conduct a full surface visual inspection data;

[0046] Figure 8 and Fig. 9 It is the first B element detection data of the semiconductor silicon wafer cleaned by the semiconductor post-sandblasting cleaning process of the present invention;

[0047] Fig.10 and Fig.11 It is the second B element detection data of the semiconductor silicon wafer cleaned by the semiconductor post-sandblasting cleaning process of the present invention;

[0048] Fig.12 and Fig.13 This is the third B element detection data of the semiconductor silicon wafer cleaned by the semiconductor post-sandblasting cleaning process of the present invention.

[0049] In the figure: 10, pre-cleaning part; 11, first tank body; 110, overflow port; 111, bubbling tube; 112, overflow tube;

[0050] 20. mortar removal part; 21. second tank body; 211. throwing bracket; 212. ultrasonic structure;

[0051] 30. Cleaning unit; 31. Third tank; 311. Spray pipe; 312. Quick exhaust valve; 32. Fourth tank; 321. Second throwing bracket; 322. Second ultrasonic structure; 33. Fifth tank;

[0052] 40. Drainer; 41. Dryer. DETAILED DESCRIPTION

[0053] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.

[0054] Figure 1 Schematic diagram of the structure of this embodiment. Figure 1As shown, this embodiment provides a semiconductor post-sandblasting cleaning system, comprising a pre-cleaning part 10, a slurry removal part 20 and a cleaning part 30 which are arranged in sequence.

[0055] The pre-cleaning unit 10 is used to clean sand particles on the surface of the silicon wafer, and includes a first tank body 11. Figure 2 Schematic diagram of the structure of the first tank body in this embodiment. Figure 2 As shown, a bubbling tube 111 is provided in each of the first tank bodies 11 .

[0056] In this embodiment, in order to facilitate the cleaning of semiconductor silicon wafers, the first trough body 11 is set as an overflow trough for accommodating water for cleaning the silicon wafers. An overflow port 110 is set at the top of the overflow trough, an overflow pipe 112 is set at the bottom, and a bubbling tube 111 is set at the bottom of the trough for introducing nitrogen bubbling to improve the cleaning effect.

[0057] The pre-cleaning section 10 is suitable for use with semiconductor silicon wafers after sandblasting, and its main purpose is to temporarily store the semiconductor silicon wafers after sandblasting, to ensure that the semiconductor silicon wafers after sandblasting are placed in clean water as soon as possible, and to ensure that the semiconductor silicon wafers are in a wet state.

[0058] When cleaning semiconductor silicon wafers, when no silicon wafer is placed in the first tank body 11, the overflow tank can be set to a small overflow state. In this embodiment, the overflow rate is set to 3L / min-5L / min. When the semiconductor silicon wafer after sandblasting is placed in the first tank body 11, the overflow rate changes to 12L / min-16L / min, and bubbling is turned on. Optionally, in this embodiment, the bubbling nitrogen flow rate is set to 150-180L / min, the pressure is 0.3Mpa, and the hole size of the bubbling tube is 0.5mm. At this flow rate, it can be ensured that large sand particles adhering to the surface of the silicon wafer are washed away.

[0059] The mortar removal part 20 is used to remove the mortar on the surface of the silicon wafer, and includes a second tank body 21, and a first cleaning agent is arranged in the second tank body 21. The first cleaning agent in this embodiment includes a high-purity HF solution, and the ratio of HF to water is 1:15.

[0060] Figure 3 Schematic diagram of the structure of the second tank body in this embodiment. Figure 3 As shown, a first tossing bracket 211, a bubbling tube and a first ultrasonic structure 212 are arranged in the second trough body 21, wherein the first tossing bracket 211 is used to shake the silicon wafer; the bubbling tube is connected to the nitrogen source for bubbling; and the first ultrasonic structure 212 is used to vibrate the silicon wafer.

[0061] In the process of removing the mortar on the surface of the silicon wafer, the silicon wafer is soaked in a high-purity HF solution to remove the natural oxide film on the surface of the silicon wafer, so as to facilitate the removal of the metal and mortar residues buried in the oxide layer. The first tossing bracket 211, the bubbling tube and the first ultrasonic structure 212 are arranged in the second tank body 21. The bubbling and tossing are to make the silicon wafer and the liquid medicine more fully. The ultrasound makes the silicon wafer vibrate, further improving the contact effect between the silicon wafer and the liquid medicine. In this embodiment, the bubbling nitrogen flow rate is 150-180L / min, the pressure is 0.3, the hole size of the bubbling tube is 0.5mm, and the swing cycle of the tossing structure is 20 times / min.

[0062] The cleaning unit 30 is used to remove surface particles and metal ions from the silicon wafer, and includes a third tank body 31 , a fourth tank body 32 and a fifth tank body 33 which are arranged in sequence.

[0063] in, Figure 4 is a schematic diagram of the structure of the third tank, such as Figure 4 As shown, the third tank body 31 adopts an overflow tank, and a spray pipe 311 and a bubbling pipe are arranged in the third tank body 31.

[0064] Specifically, the third tank body 31 is connected to a water injection pipe, a spray pipe 311 is arranged at the top of the third tank body 31 , a bubbling pipe is arranged at the bottom, and a quick exhaust valve 312 is arranged at the bottom of the third tank body 31 .

[0065] Table 1 is a table of specific working steps for the third tank

[0066] project first step Step 2 Step 3 Step 4 Step 5 Step 6 Step 7 Step 8 time 10 20 70 10 20 70 40 0 Water injection open close open open close open open close Bubbling open close close open close close open close Spray close open open close open open close close Quick sort close open close close open close close close

[0067] In this embodiment, specifically, the process time of the third tank body 31 is set to 250S.

[0068] The first step takes 10 seconds to start water injection and bubbling. The main purpose is to dissolve the HF residue on the surface of the silicon wafer into the water through bubbling.

[0069] The second step lasts for 20 seconds, with quick drain and spray turned on at the same time, in order to quickly drain the water containing HF and rinse the surface of the silicon wafer;

[0070] The third step takes 70 seconds, and pure water is added to the tank again;

[0071] Repeat steps 1 to 3 in steps 4 to 6 and rinse again;

[0072] The seventh step is to continue cleaning the silicon wafer by injecting water and bubbling. Finally, make sure that the water injection, bubbling, spraying and quick drain are all turned off.

[0073] Figure 5 is a schematic diagram of the structure of the fourth tank, such as Figure 5As shown, a second throwing bracket 321 and a second ultrasonic structure 322 are arranged in the fourth tank body 32, and a second cleaning agent is arranged in the fourth tank body 32 for oxidative cleaning of semiconductor silicon wafers.

[0074] In this embodiment, the second cleaning agent includes a mixed solution of deionized water, ammonia water, and hydrogen peroxide. The hydrogen peroxide in the solution will oxidize the surface of the silicon wafer to form a 6mm hydrophilic oxide film. The ammonia in the solution will corrode the oxide film on the surface of the silicon wafer to corrode the oxide film and take away the particles and metal on the oxide film.

[0075] The concentrations of the ammonia solution and the hydrogen peroxide solution are both 27%-32%; the volume ratio of ammonia solution: hydrogen peroxide: deionized water is 1:1:8. Specifically, the cleaning process is 130KHz ultrasound and 55-65°C for 270s. During the cleaning process, a second throwing bracket 321 is configured in the fourth tank 32, and the shaking cycle is 20 times / min. The main function is to increase the contact surface between the liquid and the silicon wafer and accelerate the reaction.

[0076] The fifth tank body 33 is configured the same as the third tank body 31 , and its process and principle are also the same as those of the third tank body 31 , which will not be described in detail here.

[0077] As an optional implementation, the present embodiment further includes a spin dryer 40, which includes at least one spin dryer 41, and the spin dryer 40 is disposed after the cleaning unit 30. The main purpose of the spin dryer 40 is to remove surface water stains from the silicon wafer by centrifugal force, so that the surface of the silicon wafer is dry.

[0078] Figure 6 It is the process flow chart of this embodiment, such as Figure 6 As shown, this embodiment also provides a semiconductor post-sandblasting cleaning process, using the semiconductor post-sandblasting cleaning system mentioned above. It includes the following steps:

[0079] S1: Pre-cleaning, used to clean sand particles on the surface of silicon wafer;

[0080] Specifically, when cleaning semiconductor silicon wafers, when no silicon wafer is placed in the first tank body 11, the overflow tank can be set to a small overflow state. In this embodiment, the overflow rate is set to 3L / min-5L / min. When the semiconductor silicon wafer after sandblasting is placed in the first tank body 11, the overflow rate changes to 12L / min-16L / min, and bubbling is turned on. Optionally, in this embodiment, the bubbling nitrogen flow rate is set to 150-180L / min, the pressure is 0.3Mpa, and the hole size of the bubbling tube is 0.5mm. At this flow rate, it can be ensured that large sand particles adhering to the surface of the silicon wafer are washed away.

[0081] S2: mortar removal, using the first cleaning agent to remove the mortar on the surface of the silicon wafer;

[0082] The first cleaning agent includes a high-purity HF solution, and the ratio of HF to water is 1:15.

[0083] The specific process is: soak the silicon wafer in high-purity HF solution to remove the natural oxide film on the surface of the silicon wafer, so as to facilitate the removal of the metal and mortar residues buried in the oxide layer. The second tank 21 is equipped with a tossing bracket 211, a bubbling tube and an ultrasonic structure 212. The bubbling and tossing are to make the silicon wafer and the liquid medicine more fully. The ultrasound makes the silicon wafer vibrate, further improving the contact effect between the silicon wafer and the liquid medicine. In this embodiment, the bubbling nitrogen flow rate is 150L / min-180L / min, the pressure is 0.3, the hole size of the bubbling tube is 0.5mm, and the swing cycle of the tossing structure is 20 times / min.

[0084] S3: Surface particle and metal ion removal, including:

[0085] S31: cleaning the first cleaning agent on the silicon wafer; referring to Table 1, specifically including:

[0086] S311: dissolving the first cleaning agent on the surface of the silicon wafer, including: injecting water into the third tank and starting bubbling for a time of not less than 10 seconds;

[0087] S312: draining the water containing the first detergent in the third tank 31, including spraying and draining, for a time of not less than 20 seconds;

[0088] S313: Re-inject pure water into the third tank 31 for a period of not less than 70 seconds;

[0089] Repeat the above steps in sequence, inject water and bubbling to continue cleaning the silicon wafer. The overall working time of step S31 is no more than 250 seconds.

[0090] S32: using a second cleaning agent to remove particles and metal ions on the surface of the silicon wafer;

[0091] Specifically, the second cleaning agent includes a mixed solution of deionized water, ammonia water and hydrogen peroxide, the concentrations of the ammonia water stock solution and the hydrogen peroxide stock solution are both 27%-32%; the volume ratio of ammonia water: hydrogen peroxide: deionized water is 1:1:8.

[0092] The specific process is: 130KHz ultrasound, 55℃-65℃ cleaning for 270s. During the cleaning process, a second oscillating bracket 321 is arranged in the fourth tank 32, and the shaking cycle is 20 times / min, which mainly increases the contact surface between the liquid and the silicon wafer and accelerates the reaction.

[0093] S33: Clean the second cleaning agent on the silicon wafer using the same process as step S31.

[0094] Specifically, referring to the first step to the eighth step in Table 1, the cleaning of the semiconductor silicon wafer is completed.

[0095] As an optional implementation, step S1: pre-cleaning, step S2: mortar removal, step S31: cleaning the first cleaning agent on the silicon wafer, and step S33: cleaning the second cleaning agent on the silicon wafer all include bubbling, wherein the bubbling nitrogen flow rate is 150L / min-180L / min; the pressure is 0.3MPa, and the diameter of the bubbling tube hole is 0.5mm.

[0096] As an optional implementation, after step S3: removing surface particles and metal ions, the present implementation further includes step S4: spin drying.

[0097] Specifically, in this embodiment, two groups of spin dryers 41 are used to perform the spin drying operation, the main purpose of which is to remove surface water stains from the silicon wafers through centrifugal force to dry the surface of the silicon wafers. In this embodiment, step S4: spin drying, the process time is 200s.

[0098] The semiconductor post-sandblasting cleaning process is used for online processing, with a daily production capacity of >7,000 pieces / day and a qualified rate of products after cleaning of >99%. Figure 7 The data was obtained by using this semiconductor sandblasting cleaning process for one week of production and performing a full surface visual inspection.

[0099] The B element detection data of the semiconductor silicon wafer cleaned by the above semiconductor sandblasting cleaning process is as follows: Figure 8 and Fig. 9 As shown in the figure, the B content after the first test data is back-sealed is qualified. Fig.10 and Fig.11 As shown in the second test data, the B content is qualified after back sealing. Fig.12 and Fig.13 As shown in the third monitoring data, the B content after back sealing is qualified.

[0100] Through the above tests, it can be known that the semiconductor post-sandblasting cleaning process can achieve a post-sandblasting cleaning yield of more than 99%, and the product metal and surface meet production requirements.

[0101] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A semiconductor post-sandblasting cleaning system, characterized in that: It includes a pre-cleaning part, a mortar removal part and a cleaning part which are arranged in sequence, wherein: The pre-cleaning part is used to clean sand particles on the surface of the silicon wafer, and includes a first tank body, and a bubbling tube is arranged in each of the first tank bodies; The mortar removal part is used to remove the mortar on the surface of the silicon wafer, and includes a second tank body, in which a first cleaning agent is arranged; The cleaning part is used to remove surface particles and metal ions from the silicon wafer, and includes a third trough body, a fourth trough body and a fifth trough body arranged in sequence, wherein a second throwing bracket and a second ultrasonic structure are arranged in the fourth trough body, and a second cleaning agent is arranged in the fourth trough body, and the third trough body and the fifth trough body are both provided with a spray pipe and a bubbling pipe.

2. The semiconductor post-sandblasting cleaning system according to claim 1, characterized in that: A first tossing bracket, a bubbling tube and a first ultrasonic structure are arranged in the second tank body, wherein the first tossing bracket is used to shake the silicon wafer; the bubbling tube is connected to a nitrogen source for bubbling; and the first ultrasonic structure is used to vibrate the silicon wafer.

3. The semiconductor post-sandblasting cleaning system according to claim 1, characterized in that: The first tank body, the third tank body and the fifth tank body all adopt overflow tanks.

4. The semiconductor post-sandblasting cleaning system according to any one of claims 1 to 3, characterized in that: The first cleaning agent includes a high-purity HF solution, and the ratio of HF to water is 1:

15.

5. The semiconductor post-sandblasting cleaning system according to any one of claims 1 to 3, characterized in that: The second cleaning agent includes a mixed solution of deionized water, ammonia water, and hydrogen peroxide, wherein: The concentrations of ammonia solution and hydrogen peroxide solution are both 27%-32%; The volume ratio of ammonia water: hydrogen peroxide: deionized water is 1:1:

8.

6. The semiconductor post-sandblasting cleaning system according to any one of claims 1 to 3, characterized in that: It also includes a spin drying section, which includes at least one spin dryer and is arranged after the cleaning section.

7. A semiconductor post-sandblasting cleaning process, characterized in that: The semiconductor post-sandblasting cleaning system according to any one of claims 1 to 6 comprises the following steps: S1: Pre-cleaning, used to clean sand particles on the surface of silicon wafer; S2: removing mortar, using the first cleaning agent to remove the mortar on the surface of the silicon wafer; S3: Surface particle and metal ion removal, including: S31: cleaning the first cleaning agent on the silicon wafer; S32: using the second cleaning agent to remove particles and metal ions on the surface of the silicon wafer; S33: Cleaning the second cleaning agent on the silicon wafer using the same process as step S31.

8. The semiconductor post-sandblasting cleaning process according to claim 7, characterized in that: Step S31: cleaning the first cleaning agent on the silicon wafer, comprising: Dissolving the first cleaning agent on the surface of the silicon wafer, including: injecting water into the third tank and starting bubbling for a time of not less than 10 seconds; draining the water containing the first cleaning agent in the third tank, including spraying and draining, for a period of not less than 20 seconds; Re-injecting pure water into the third tank body for a period of not less than 70 seconds; The above steps are repeated in sequence, water is injected and bubbling is performed to continue cleaning the silicon wafer, and the overall working time of step S31 is no more than 250 seconds.

9. The semiconductor post-sandblasting cleaning process according to claim 7, characterized in that: Step S1: pre-cleaning, step S2: slurry removal, step S31: cleaning the first cleaning agent on the silicon wafer, and step S33: cleaning the second cleaning agent on the silicon wafer, all include bubbling, wherein: The bubbling nitrogen flow rate is 150L / min-180L / min; the pressure is 0.3MPa, and the diameter of the bubbling tube hole is 0.5mm.

10. The semiconductor post-sandblasting cleaning process according to claim 7, characterized in that: Step S32: using the second cleaning agent to remove particles and metal ions on the surface of the silicon wafer, including: Use 130KHz ultrasound and clean at 55℃-65℃ for no less than 270s; The silicon wafer is polished while being cleaned, with a polishing cycle of 20 times / min.

Citation Information

Patent Citations

  • Cleaning method for removing the optical resistance residue and dual enchasing technology of the copper making process

    CN101055849A

  • Cut / ground silicon wafer surface cleaning apparatus

    CN102412173A

  • Efficient cleaning device and cleaning method for wafers

    CN109201608A

  • Cleaning method for reducing metal and particles on surface of silicon wafer after adhesive tape grinding

    CN115863147A

  • Method for cleaning metal residues on surface of silicon carbide wafer

    CN115995379A