Surface treatment method for multicolor moissi diamonds

Through a multi-step method combining ultrasonic cleaning, high-temperature annealing, inert gas treatment and ion energy radiation, the problem of immature surface treatment of multi-color moissanite is solved, the surface cleanliness and alkali resistance is improved, and environmental pollution is reduced risk.

CN119016467APending Publication Date: 2024-11-26GUANGXI XIHUI TIANCHENG TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411133718.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the surface treatment process for multi-color moissanite drills is immature, and it is difficult to effectively remove surface impurities and contaminants, and there is environmental impact and corrosion risks in chemical treatment.

Method used

The combined methods of ultrasonic cleaning, high-temperature annealing, inert gas treatment and ion energy radiation treatment are adopted, combined with the prepared potassium hydroxide ethanol solution washing liquid, surface impurities and contaminants are gradually removed, and surface smoothness and alkali resistance are improved.

Benefits of technology

Effectively remove surface impurities and pollutants, improve the translucency and wear resistance of Moissanite, reduce roughness, improve alkali resistance, and reduce environmental pollution risks.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a multicolor Momulberry diamond surface treatment method which comprises the following steps: step 1, putting Momulberry diamond into an ultrasonic cleaning instrument, adding a proper amount of plasma water, cleaning for 1-2 hours under the ultrasonic power of 10-40W, taking out after cleaning, and air-drying until the water content is 3-7%; high-temperature annealing is carried out on the moissimus diamonds, so that impurities near the surface of the moissimus diamonds can be effectively removed, and meanwhile, the moissimus diamonds become transparent through color fixation. The method comprises the following steps: step 1, preparing a cleaning solution, placing momulberry diamonds into high-purity inert gas (N2, Ar and the like) for heating treatment at the heating temperature of 150-250 DEG C for 25-30 min, step 2, placing momulberry diamonds into the prepared cleaning solution for treatment at the treatment temperature of 60-80 DEG C for 1-2 h, after treatment is completed, performing surface irradiation treatment, and finally drying.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of moissanite processing, and in particular to a surface processing method for multi-color moissanite. Background Art

[0002] Moissanite is synthetic silicon carbide, which looks similar to diamonds and is even more dazzling than diamonds. To distinguish the two, you need to use professional instruments to carefully observe the internal structure. Moissanite is only slightly lower in hardness than diamonds, but its refractive index and brightness are higher than diamonds. Therefore, moissanite is the most shining gem in the world. Moissanite is loved by women for its beauty comparable to diamonds and its relatively low price. It is very popular in the Japanese, Korean, European and American markets.

[0003] Surface treatment is a process that uses physical and chemical modifications on the base material to make the surface of the material different from the internal mechanical, physical and chemical properties. Generally speaking, the purpose of surface treatment is to enhance the corrosion resistance, wear resistance and flatness of the material surface.

[0004] Physical treatment is generally a treatment method that improves the smoothness of materials through mechanical friction and cutting. The advantages are simple operation and little pollution to the environment. The disadvantages are also very obvious, that is, large wear and tear of materials. Chemical treatment is to achieve the purpose of modifying the surface of materials through chemical reactions between acidic or alkaline reagents and oxides and oil stains on the surface of materials. However, chemical treatment is complicated to operate, and if it is not operated properly, it may cause corrosion damage to the precision parts of the workpiece. Secondly, chemical treatment has a great impact on the environment. Therefore, in practice, a process combining physical treatment and chemical treatment is often used.

[0005] There are few existing documents on the surface treatment of multi-color moissanite, that is, the surface treatment of moissanite is still in an immature stage. Therefore, the present invention proposes a surface treatment method for multi-color moissanite. Summary of the invention

[0006] The present invention aims to provide a surface treatment method for multi-color moissanite to solve the problems that need to be solved urgently in the above background.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A method for surface treatment of multi-color moissanite, the operation steps are as follows:

[0009] Step 1: Place the pre-processed moissanite in an ultrasonic cleaner, add an appropriate amount of plasma water and clean for 1-2 hours with an ultrasonic power of 10-40W to preliminarily remove surface impurities. After cleaning, take it out and air dry it naturally until the water content is 3%-7%.

[0010] Step 2: Place the moissanite in a tubular furnace and heat it to 100℃-200℃. Keep it warm for 1-2 hours and then cool it to room temperature in the furnace. High-temperature annealing of moissanite can effectively remove impurities near the surface and fix the color to make it transparent. Then place the moissanite in a high-purity inert gas (N2, Ar, etc.) for heating. The heating temperature is 150℃-250℃ for 25min-30min.

[0011] Step 3: Place the moissanite in the prepared washing liquid for treatment at a temperature of 60℃-80℃ for 1-2 hours. After the treatment, perform surface irradiation treatment. Finally, dry it in a drying oven at a temperature of about 50℃ for 20-40 minutes.

[0012] As a further solution of the present invention, the preparation method of the washing liquid is to take 100g of potassium hydroxide, dissolve it in 50ml of water, and then add industrial ethanol to 1L to prepare an ethanol solution of potassium hydroxide. It is suitable for washing surface pollutants such as grease, resin, etc. on moissanite: this strong alkaline washing liquid is very corrosive to glassware, and the washing time should not be too long, and it should be used with caution.

[0013] As a further solution of the present invention, the surface irradiation treatment is performed by using a mixed ion beam with an ion energy of 200-300ev, a beam current density of 150-170A / cm2, and a pulse width of 50-60ns, and the treatment time is 5-10s.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] The present invention firstly performs ultrasonic water washing to preliminarily remove the easily cleaned surface impurities. After high temperature annealing, the near-surface impurities inside the moissanite are removed and the color is fixed to make it more transparent. Then, the moissanite surface structure undergoes sparse denaturation after high temperature treatment with inert gas. Then, the surface is flattened by plasma irradiation to remove impurities. Finally, the surface is cleaned with a prepared washing liquid to remove pollutants. DETAILED DESCRIPTION

[0016] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Of course, the following examples are only some examples of the present invention, not all implementation plans. Based on the actual cases in the present invention, all other implementation cases obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0017] Embodiment 1:

[0018] A multi-color moissanite surface treatment method of this embodiment includes the following steps:

[0019] Step 1: Place the pre-processed moissanite in an ultrasonic cleaner, add an appropriate amount of plasma water and clean for 1 hour, with an ultrasonic power of 10W to preliminarily remove surface impurities. After cleaning, take it out and air dry it naturally to a moisture content of 3%.

[0020] Step 2: Then put it into a tube furnace and heat it to 100°C. Keep it warm for 1 hour and then cool it to room temperature in the furnace. Then put it in an argon atmosphere for heating treatment. The heating temperature is 150°C and the heating time is 25 minutes.

[0021] Step 3: Place the moissanite in the prepared washing liquid for treatment at 60°C for 1 hour. After the treatment, perform surface irradiation treatment. Finally, dry it in a drying oven at 50°C for 20 minutes.

[0022] As a further solution of the present invention, the preparation method of the washing liquid is to take 100g of potassium hydroxide, dissolve it in 50ml of water, and then add industrial ethanol to 1L to prepare an ethanol solution of potassium hydroxide.

[0023] As a further solution of the present invention, the surface irradiation treatment is performed by using a mixed ion beam with an ion energy of 200 ev, a beam current density of 150 A / cm2, and a pulse width of 50 ns, and the treatment time is 5 s.

[0024] Embodiment 2:

[0025] A multi-color moissanite surface treatment method of this embodiment includes the following steps:

[0026] Step 1: Place the pre-processed moissanite in an ultrasonic cleaner, add an appropriate amount of plasma water and clean for 1.5 hours with an ultrasonic power of 15W to preliminarily remove surface impurities. After cleaning, take it out and air dry it naturally to a moisture content of 5%.

[0027] Step 2: Then put it into a tube furnace and heat it to 150℃. Keep it warm for 1.5 hours and then cool it to room temperature in the furnace. Then put it in an argon atmosphere for heating treatment. The heating temperature is 200℃ and the heating time is 30 minutes.

[0028] Step 3: Place the moissanite in the prepared washing liquid for treatment at 70°C for 1.5 hours. After the treatment, perform surface irradiation treatment. Finally, dry it in a drying oven at 50°C for 30 minutes.

[0029] As a further solution of the present invention, the preparation method of the washing liquid is to take 100g of potassium hydroxide, dissolve it in 50ml of water, and then add industrial ethanol to 1L to prepare an ethanol solution of potassium hydroxide.

[0030] As a further solution of the present invention, the surface irradiation treatment is performed by using an ion beam with an ion energy of 250 ev, a beam current density of 160 A / cm2, and a pulse width of 55 ns, and the treatment time is 7 s.

[0031] Embodiment 3:

[0032] A multi-color moissanite surface treatment method of this embodiment includes the following steps:

[0033] Step 1: Place the pre-processed moissanite in an ultrasonic cleaner, add an appropriate amount of plasma water and clean for 2 hours, with an ultrasonic power of 20W to preliminarily remove surface impurities. After cleaning, take it out and air dry it naturally to a moisture content of 6%.

[0034] Step 2: Then put it into a tube furnace and heat it to 200℃. Keep it warm for 2h and then cool it to room temperature in the furnace. Then put it in an argon atmosphere for heating treatment. The heating temperature is 250℃ and the heating time is 30min.

[0035] Step 3: Place the moissanite in the prepared washing liquid for treatment at 80°C for 2 hours. After the treatment, perform surface irradiation treatment. Finally, dry it in a drying oven at 50°C for 40 minutes.

[0036] As a further solution of the present invention, the preparation method of the washing liquid is to take 100g of potassium hydroxide, dissolve it in 50ml of water, and then add industrial ethanol to 1L to prepare an ethanol solution of potassium hydroxide.

[0037] As a further solution of the present invention, the surface irradiation treatment is performed by using an ion beam with an ion energy of 300 ev, a beam current density of 170 A / cm2, and a pulse width of 60 ns, and the treatment time is 10 s.

[0038] Comparative Example 1:

[0039] The materials and preparation process are basically the same as those in Example 3, the only difference being that the prepared washing liquid is not used for treatment.

[0040] Comparative Example 2:

[0041] The materials and preparation process are basically the same as those in Example 3, the only difference being that the materials have not been irradiated by plasma.

[0042] Case Roughness(um) Alkali resistance (d) Example 1 0.13 295 Example 2 0.11 297 Example 3 0.08 303 Comparative Example 1 0.16 270 Comparative Example 2 0.20 285

[0043] Example 3 of the present invention has a roughness of 0.08um and an alkali resistance of 303d. In Comparative Example 1, no prepared washing liquid was used for treatment, and the roughness was 0.16um and the alkali resistance was 270d. Compared with Comparative Example 1, the roughness of Example 3 was reduced by 0..08, the improvement rate was 50%, and the alkali resistance was increased by 33d, an increase of 12.2%.

[0044] In Example 3 of the present invention, the roughness is 0.08um and the alkali resistance is 303d. In Comparative Example 2, plasma irradiation is not used, the roughness is 0.20um, and the alkali resistance is 285d. Compared with Comparative Example 2, the roughness of Example 3 is reduced by 0.12, the improvement rate is 60%, and the alkali resistance is increased by 18d, an increase of 6.3%.

[0045] It is obvious to those skilled in the art that the present invention is not limited to the exemplary details of the above examples, and other specific operations may be used to implement the present invention without violating the spirit or essential features of the present invention. Therefore, the above examples are exemplary rather than restrictive, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.

[0046] In addition, it can be understood that although the present invention is described according to implementation modes, not every implementation mode has only one independent technical solution. The description in the specification is only for the sake of clarity. Those skilled in the art should regard the present invention as a whole. The technical solutions in each embodiment can also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for surface treatment of multi-color moissanite, characterized in that: The following steps are included: Step 1: Place the pre-processed moissanite in an ultrasonic cleaner, add an appropriate amount of plasma water and clean for 1-2 hours with an ultrasonic power of 10-40W to preliminarily remove surface impurities. After cleaning, take it out and air dry it naturally until the water content reaches 3%-7%; Step 2: Place the moissanite in a tubular furnace, heat it to 100℃-200℃, keep it warm for 1-2h, and then cool it to room temperature in the furnace. High-temperature annealing of the moissanite can effectively remove impurities near the surface, and fix the color to make the moissanite transparent. Then place the moissanite in a high-purity inert gas (N2 and Ar) for heating treatment at 150℃-250℃ for 25min-30min. Step 3: Place the moissanite in the prepared washing liquid for treatment at a temperature of 60℃-80℃ for 1-2h. After the treatment, perform surface irradiation treatment and finally dry it in a drying oven at a temperature of about 50℃ for 20-40min.

2. A multi-color moissanite surface treatment method according to claim 1, characterized in that: The preparation method of the washing liquid is as follows: 100g of potassium hydroxide is taken, dissolved in 50ml of water, and then industrial ethanol is added to 1L to prepare an ethanol solution of potassium hydroxide.

3. The method for surface treatment of multi-color moissanite according to claim 1, characterized in that: The surface irradiation treatment is performed by using a mixed ion beam with an ion energy of 200-300 ev, a beam current density of 150-170 A / cm2, and a pulse width of 50-60 ns, and the treatment time is 5-10 s.

Citation Information

Patent Citations

  • Method for depositing silicon carbide high radiation coating on cobalt based high-temperature alloy surface

    CN101343731A

  • Ultrasonic-vibration activation-assisted sintering tubular furnace

    CN104180654A

  • Moissanite surface treatment technology

    CN109849202A

  • Method for depositing diamond film coating on surface of moissanite

    WO2023035429A1