Control method and device for eliminating strip steel edge yield line defect, medium and equipment

By real-time detection of strip edge thickness and adjustment of cold rolling mill parameters during cold rolling, the problem of edge yield marks during strip annealing after cold rolling was solved, achieving efficient defect prediction and elimination, and improving yield and production efficiency.

CN119016522APending Publication Date: 2024-11-26SHOUGANG ZHIXIN QIAN AN ELECTROMAGNETIC MATERIALS CO LTD

Patent Information

Application Number
CN202411166456.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Cold-rolled strip steel is prone to edge yield marks after annealing, which leads to yield loss and is difficult to predict. Existing technologies cannot detect and deal with these defects in a timely manner.

Method used

During the cold rolling process, the edge thickness of the strip is monitored in real time. By adjusting the working roll shifting and bending values ​​of the cold rolling mill, the edge thickness is made smaller than the middle thickness, thus predicting and eliminating possible edge yield marks after annealing.

Benefits of technology

Predicting and eliminating yield marks on the edges of strip steel in advance ensures strip quality and shape, improves production line efficiency and yield, and reduces resource waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016522A_ABST
    Figure CN119016522A_ABST
Patent Text Reader

Abstract

The invention provides a control method and device for eliminating strip steel edge yield line defects, a medium and equipment, and the method comprises the steps that the edge thickness of strip steel is detected in real time based on strip steel point positions of the strip steel; if it is continuously detected that the edge thickness is larger than the middle thickness of the strip steel and the number of continuous strip steel point positions exceeds the preset number, it is pre-judged that the strip steel has the edge yield line defect after annealing treatment; adjusting the roll shifting value of a working roll of the cold-rolling mill to enable the side thickness to be smaller than the middle thickness; and if the accumulated adjustment value of the working roll shifting value reaches a first preset value and the edge thickness is larger than or equal to the middle thickness, the working roll bending value of the cold rolling mill is adjusted, so that the edge thickness is smaller than the middle thickness. In the strip steel cold rolling process, the edge thickness of the strip steel can be controlled to be smaller than the middle thickness of the strip steel, the edge yield line defect of the strip steel can be eliminated, the strip shape and quality of the strip steel are guaranteed, and the production efficiency of a production line and the strip steel yield are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of steel rolling, and in particular to a control method, device, medium and equipment for eliminating yield line defects at the edge of a steel strip. Background Art

[0002] After cold rolling, thin-gauge, low-strength strip steel will generate internal stress at the edge of the strip steel. Large internal stress will manifest as wave-shaped defects such as middle waves, edge waves, rib waves, and compound waves. In order to eliminate the wave shape, the cold-rolled strip steel needs to be annealed to eliminate internal stress and reduce the yield strength to facilitate subsequent processing. When the rolled strip steel is annealed, the internal stress at the edge of the strip steel is superimposed on the tension applied to the strip steel by the furnace roller, causing the strip steel to yield, resulting in edge yield line defects on the edge of the strip steel. After such defects occur, the defective parts need to be resected, resulting in a loss of yield rate and the inability to honor the original order. In addition, since such defects can only be discovered after annealing, they are very likely to cause batch defects, resulting in huge manufacturing losses.

[0003] Based on this, how to adopt an effective control method to eliminate the edge yield line defects of the strip, so as to predict in advance whether the strip will have edge yield line defects after annealing, and take improvement measures in time to eliminate the edge yield line defects of the strip, ensure the plate shape and quality of the strip, and improve the production efficiency of the production line and the yield rate of the strip, is a technical problem that needs to be solved urgently. Summary of the invention

[0004] The purpose of the present application is to provide a control method, device, medium and equipment for eliminating edge yield line defects of strip steel. The present application solves the problem of edge yield line defects of cold-rolled strip steel after annealing. During the cold rolling process of the strip steel, the present application can control the edge thickness of the strip steel to be less than the middle thickness of the strip steel, so as to predict in advance whether the strip steel will have edge yield line defects in subsequent annealing treatment, and adjust the cold rolling parameters in time to eliminate the edge yield line defects of the strip steel, ensure the plate shape and quality of the strip steel, and improve the production efficiency of the production line and the yield rate of the strip steel.

[0005] Specifically, this application adopts the following technical solutions:

[0006] According to one aspect of an embodiment of the present application, a control method for eliminating yield line defects on the edge of a steel strip is provided, the method comprising: in a process of cold rolling the steel strip, detecting the edge thickness of the steel strip in real time based on the strip points of the steel strip; if it is continuously detected that the edge thickness is greater than the middle thickness of the steel strip, and the number of continuous strip points exceeds a preset number, predicting that the steel strip has an edge yield line defect after annealing; adjusting the working roll shifting value of the cold rolling mill so that the edge thickness is less than the middle thickness; if the edge thickness is greater than or equal to the middle thickness after the cumulative adjustment value of the working roll shifting value reaches a first preset value, adjusting the working roll bending value of the cold rolling mill so that the edge thickness is less than the middle thickness.

[0007] In some embodiments of the present application, based on the aforementioned solution, a strip profile detection device is installed on the cold rolling production line to detect the edge thickness of the strip in real time based on the strip position of the strip.

[0008] In some embodiments of the present application, based on the aforementioned scheme, the adjusting of the working roll shifting value of the cold rolling mill so that the edge thickness is smaller than the middle thickness includes: adjusting the working roll shifting value multiple times, and in each adjustment, the working roll shifting value is increased by 3 mm until the edge thickness is smaller than the middle thickness or the cumulative adjustment value of the working roll shifting value reaches a first preset value.

[0009] In some embodiments of the present application, based on the aforementioned solution, the preset number is 5.

[0010] In some embodiments of the present application, based on the aforementioned solution, the first preset value is 15 mm.

[0011] In some embodiments of the present application, based on the aforementioned scheme, the adjusting of the working roll bending value of the cold rolling mill so that the edge thickness is smaller than the middle thickness includes: adjusting the working roll bending value multiple times, and in each adjustment, the working roll bending value is reduced by 0.5 tons until the edge thickness is smaller than the middle thickness, and the cumulative adjustment value of the working roll bending value is a second preset value.

[0012] In some embodiments of the present application, based on the aforementioned solution, the second preset value is 4 tons.

[0013] According to one aspect of an embodiment of the present application, a control device for eliminating yield line defects on the edge of a steel strip is provided, the device comprising: a detection unit, which is used to detect the edge thickness of the steel strip in real time based on the strip points of the steel strip during cold rolling of the steel strip; a prejudgment unit, which is used to prejudge that the steel strip has edge yield line defects after annealing if it is continuously detected that the edge thickness is greater than the middle thickness of the steel strip and the number of continuous strip points exceeds a preset number; a first adjustment unit, which is used to adjust the working roll shifting value of the cold rolling mill so that the edge thickness is less than the middle thickness; and a second adjustment unit, which is used to adjust the working roll bending value of the cold rolling mill so that the edge thickness is less than the middle thickness if the edge thickness is greater than or equal to the middle thickness after the cumulative adjustment value of the working roll shifting value reaches a first preset value.

[0014] According to one aspect of an embodiment of the present application, a computer-readable storage medium is provided, in which at least one program code is stored. The at least one program code is loaded and executed by a processor to implement the operations performed by the above-mentioned control method for eliminating yield line defects on the edge of strip steel.

[0015] According to one aspect of an embodiment of the present application, an electronic device is provided, including a memory and a processor, wherein the memory stores a computer program, and the processor executes the computer program to implement the operations performed by the above-mentioned control method for eliminating yield line defects on the edge of a strip.

[0016] It can be seen from the above technical solution that the present application has at least the following advantages and positive effects:

[0017] The solution proposed in the present application can solve the problem of edge yield line defects in cold-rolled strip after annealing. During the cold rolling process of the strip, the present application can control the edge thickness of the strip to be smaller than the middle thickness of the strip, so as to predict in advance whether the strip will have edge yield line defects in the subsequent annealing treatment, and adjust the cold rolling parameters in time to eliminate the edge yield line defects of the strip, ensure the plate shape and quality of the strip, and improve the production efficiency of the production line and the yield rate of the strip. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions in the present application, the following is a brief introduction to the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0019] Figure 1 A flow chart of a control method for eliminating yield line defects at the edge of a steel strip in one embodiment of the present application is shown;

[0020] Figure 2 A schematic diagram of a cold rolling mill roll system in one embodiment of the present application is shown;

[0021] Figure 3 A structural block diagram of a control device for eliminating yield line defects at the edge of a steel strip in one embodiment of the present application is shown;

[0022] Figure 4 A schematic diagram of the structure of a computer system suitable for implementing an electronic device of an embodiment of the present application is shown. DETAILED DESCRIPTION

[0023] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the examples set forth herein; rather, these embodiments are provided so that this application will be more comprehensive and complete and fully convey the concept of the example embodiments to those skilled in the art.

[0024] In addition, described feature, structure or characteristic can be combined in one or more embodiments in any suitable manner. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present application. However, those skilled in the art will appreciate that the technical scheme of the present application can be put into practice without one or more of the specific details, or other methods, components, devices, steps, etc. can be adopted. In other cases, known methods, devices, realizations or operations are not shown or described in detail to avoid blurring the various aspects of the application.

[0025] The flowcharts shown in the accompanying drawings are only exemplary and do not necessarily include all the contents and operations / steps, nor must they be executed in the order described. For example, some operations / steps can be decomposed, and some operations / steps can be combined or partially combined, so the actual execution order may change according to actual conditions.

[0026] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the objects used in this way can be interchanged where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those shown or described.

[0027] During the cold rolling process of thin and low-strength strip steel, due to lubrication, friction, shape control, deformation temperature and other reasons, internal stress will be generated inside the strip steel after rolling. Large internal stress will appear as wave-shaped defects such as middle wave, edge wave, rib wave and compound wave on the strip steel shape. In order to eliminate the wave shape, the cold-rolled strip steel needs to be annealed to eliminate the internal stress and reduce the yield strength of the strip steel for subsequent processing.

[0028] During the annealing process of thin-gauge and low-strength strip steel, due to the high temperature of the annealing furnace, the strip steel is also affected by tension during annealing in the furnace. When the internal stress of the strip steel after rolling is eliminated, it is very easy to have a transversely distributed edge yield line defect on the edge of the strip steel after annealing. The defect is concentrated on both sides of the edge of the strip steel. The distribution depth of the edge yield line defect extends from both sides of the edge of the strip steel to the middle of the strip steel within 100mm. The distribution direction of the edge yield line defect is perpendicular to the rolling direction or distributed at 45°, showing an obvious yield extension shape. When the edge yield line defect appears in the strip steel, the part where the edge yield line defect occurs needs to be recut for the second time, which greatly causes the loss of the yield rate and the original order cannot be fulfilled. In addition, since such defects can only be found after annealing, but the root cause of such defects is caused by the cold rolling process, it cannot be found in time, which is very easy to cause batch defects, resulting in great losses.

[0029] In order to solve the above problems, the present application proposes a control method, device, medium and equipment for eliminating the edge yield line defect of the steel strip. The present application detects the edge thickness of the steel strip in real time during the cold rolling process to predict whether the steel strip will have edge yield line defects after annealing. If it is predicted that the edge of the steel strip will have edge yield line defects after annealing, the rolling parameters of the cold rolling mill are adjusted to avoid the edge yield line defects on the edge of the steel strip after annealing, thereby ensuring the shape and quality of the steel strip and improving the production efficiency of the production line and the yield rate of the steel strip.

[0030] The implementation details of the technical solution of the embodiment of the present application are described in detail below:

[0031] Reference Figure 1 , Figure 1 This is a flow chart of a control method for eliminating yield line defects at the edge of a steel strip in one embodiment of the present application.

[0032] According to a typical embodiment of the present application, a control method for eliminating yield line defects at the edge of a strip is provided, and the method includes the following steps S1 to S4:

[0033] Step S1, during the cold rolling process of the steel strip, the edge thickness of the steel strip is detected in real time based on the strip position of the steel strip.

[0034] In one embodiment of the present application, a strip profile detection device installed in a cold rolling production line can be used to detect the edge thickness of the strip in real time based on the strip position of the strip.

[0035] Step S2: If it is continuously detected that the edge thickness is greater than the middle thickness of the strip, and the number of continuous strip points exceeds a preset number, it is predicted that the strip has an edge yield line defect after annealing.

[0036] In the present application, during the cold rolling of the steel strip, the edge thickness of the steel strip can be detected in real time based on the strip point of the steel strip, and the edge thickness can be the thickness of the edges on both sides of the steel strip in the width direction. It is understandable that during the cold rolling of the steel strip, due to the influence of various external environments, the rolling parameters of the cold rolling mill will deviate, resulting in uneven extension of the steel strip in the width direction, small extension of the edges and large extension of the middle, resulting in internal stress of tensile stress at the edges of the steel strip. When the rolled steel strip is annealed, the internal stress of the edge of the steel strip is superimposed on the tension applied to the steel strip by the furnace rollers in the annealing furnace, causing the steel strip to yield, resulting in edge yield line defects at the edges of the steel strip after annealing.

[0037] Since the fundamental reason for the existence of edge yield line defects on the edge of the strip is the unreasonable rolling parameters during the cold rolling process, which makes the edge thickness of the strip greater than the middle thickness of the strip, in order to avoid the existence of the edge yield line defects on the strip after annealing, it is necessary to detect the edge thickness of the strip in real time to control the edge thickness to be less than the middle thickness. When the edge thickness of the strip is detected in real time based on the strip points of the strip, if it is only accidentally detected that the edge thickness of a strip point is greater than the middle thickness, it cannot be used as a condition for predicting the existence of edge yield line defects on the strip after annealing. It may be because the detection device obtains abnormal data or other external factors (such as rolling mill vibration, strip deviation, etc.), resulting in the phenomenon that the edge thickness of a strip point is greater than the middle thickness.

[0038] In order to avoid the influence of accidental factors when detecting the edge thickness of the steel strip, when the edge thickness of the steel strip is detected in real time based on the strip points of the steel strip, if the edge thickness is continuously detected to be greater than the middle thickness of the steel strip, and the number of continuous strip points exceeds a preset number, it is predicted that the steel strip has an edge yield line defect after annealing. It is limited that the edge thickness needs to be continuously detected to be greater than the middle thickness, and the number of continuous strip points must exceed a preset number before it is predicted that the steel strip will have an edge yield line defect after annealing, which greatly improves the accuracy of the edge thickness detection of the steel strip and avoids the occurrence of false detection.

[0039] In the present application, the strip profile detection device installed in the cold rolling production line can detect the edge thickness of the strip in real time based on the strip points of the strip. The strip profile detection device can detect the thickness of different strip points of the strip through multiple X-RAYs, and then couple the profile of the strip to determine the strip profile. When it is found that within 200mm from the edge of the strip, the edge thickness is continuously detected to be greater than the middle thickness of the strip, and the number of continuous strip points exceeds the preset number, it is predicted that the strip has an edge yield line defect after annealing, and a system warning is issued at the same time to remind the operator that the strip edge thickness is abnormal. The distribution depth of the edge yield line defect extends within 100 mm from both sides of the edge of the strip to the middle of the strip, but the strip contour detection device can detect the thickness of the strip points within 200 mm from the edge of the strip. The strip contour detection device can detect once every 200 milliseconds, which greatly improves the accuracy of strip edge thickness detection and also improves the accuracy of predicting whether the strip has edge yield line defects after annealing.

[0040] In one embodiment of the present application, the preset number can be 5, 6 or other numbers. The present application does not impose any special restrictions on this and the preset number can be adjusted according to actual production needs. It can be understood that the more the preset number, the higher the detection accuracy of the strip profile detection device.

[0041] Step S3, adjusting the working roll shifting value of the cold rolling mill so that the edge thickness is smaller than the middle thickness.

[0042] In one embodiment of the present application, adjusting the working roll shifting value of the cold rolling mill so that the edge thickness is smaller than the middle thickness includes:

[0043] The working roll shifting value is adjusted multiple times, and in each adjustment, the working roll shifting value is increased by 3 mm until the edge thickness is less than the middle thickness or the cumulative adjustment value of the working roll shifting value reaches a first preset value.

[0044] In one embodiment of the present application, the first preset value may be 15 mm. The first preset value may also be other values. The present application does not impose any special restrictions on this. The first preset value may be adjusted according to actual production needs.

[0045] In the present application, after predicting that the strip has edge yield line defects after annealing, in order to avoid the edge yield line defects in the strip during the subsequent annealing process, the rolling parameters of the cold rolling mill need to be adjusted in time. Figure 2 , Figure 2 A schematic diagram of a cold rolling mill roll system in an embodiment of the present application is shown, wherein the cold rolling mill may include an upper support roll 201 , a lower support roll 202 , an upper intermediate roll 203 , a lower intermediate roll 204 , an upper working roll 205 , and a lower working roll 206 . When adjusting the rolling parameters of the cold rolling mill, the working roll shifting value can be adjusted multiple times first. The specific adjustment can be determined according to the edge thickness of the strip. If the strip thickness is that the edge thickness of the strip on the working side is greater than the middle thickness of the strip, the upper working roll shifting value of the upper working roll 205 is adjusted multiple times. In each adjustment, the upper working roll shifting value is increased by 3mm until the edge thickness of the strip on the working side is less than the middle thickness of the strip or the cumulative adjustment value of the upper working roll shifting value reaches 15mm; if the strip thickness is that the edge thickness of the strip on the driving side is greater than the middle thickness of the strip, the lower working roll shifting value of the lower working roll 206 is adjusted multiple times. In each adjustment, the lower working roll shifting value is increased by 3mm until the edge thickness of the strip on the driving side is less than the middle thickness of the strip or the cumulative adjustment value of the lower working roll shifting value reaches 15mm.

[0046] Step S4: If the edge thickness is greater than or equal to the middle thickness after the cumulative adjustment value of the working roll shifting value reaches a first preset value, the working roll bending value of the cold rolling mill is adjusted so that the edge thickness is less than the middle thickness.

[0047] In one embodiment of the present application, the step of adjusting the bending value of the working roll of the cold rolling mill so that the edge thickness is smaller than the middle thickness comprises:

[0048] The working roll bending value is adjusted multiple times. In each adjustment, the working roll bending value is reduced by 0.5 tons until the edge thickness is less than the middle thickness. The cumulative adjustment value of the working roll bending value is a second preset value.

[0049] In one embodiment of the present application, the second preset value may be 4 tons. When the working roll bending value is adjusted multiple times, the cumulative adjustment value of the working roll bending value may be 4 tons. The second preset value may also be other values. The present application does not impose any special restrictions on this. The second preset value may be adjusted according to the actual production needs. It should be noted here that if the edge thickness is already less than the middle thickness during the process of adjusting the working roll shifting value multiple times and the cumulative adjustment value of the working roll shifting value does not reach the first preset value, then the working roll bending value does not need to be adjusted. If the edge thickness is still greater than or equal to the middle thickness after the cumulative adjustment value of the working roll shifting value reaches the first preset value, the working roll bending value of the cold rolling mill needs to be adjusted so that the edge thickness is less than the middle thickness. In the process of adjusting the working roll bending value multiple times, the edge thickness can be made less than the middle thickness. There will be no situation where the edge thickness is still greater than or equal to the middle thickness after the cumulative adjustment value of the working roll bending value reaches the second preset value (4 tons).

[0050] In the present application, after the working roll shifting value is adjusted multiple times and the cumulative adjustment value of the working roll shifting value reaches the first preset value (15 mm), if the edge thickness is still greater than or equal to the middle thickness, the working roll bending value needs to be adjusted multiple times, and reference can be made to Figure 2 , the working roll bending value may include an upper working roll bending value of an upper working roll 205 and a lower working roll bending value of a lower working roll 206. When the working roll bending value is adjusted multiple times, the specific adjustment may be determined according to the edge thickness of the strip. If the strip thickness is that the edge thickness of the strip on the working side is greater than or equal to the middle thickness of the strip, the upper working roll bending value is adjusted multiple times, and in each adjustment, the upper working roll bending value is reduced by 0.5 tons until the edge thickness is less than the middle thickness; if the strip thickness is that the edge thickness of the strip on the driving side is greater than the middle thickness of the strip, the lower working roll bending value of the lower working roll 206 is adjusted multiple times, and in each adjustment, the lower working roll bending value is reduced by 0.5 tons until the edge thickness is less than the middle thickness.

[0051] In this application, reference is made to Figure 2Since the upper intermediate roll 203, the lower intermediate roll 204, the upper working roll 205, and the lower working roll 206 of the cold rolling mill all have roll cones, when the strip is cold rolled, the upper roll system and the lower roll system both apply rolling force to the strip. Due to the influence of the roll cones, the middle parts of the upper working roll 205 and the lower working roll 206 will bend in the direction of the rolling force, resulting in the rolling force on the middle part of the strip being greater than the rolling force on the edge of the strip, making the strip thin in the middle and thick at the edge. When the working roll bending value is adjusted multiple times, taking the case where the edge thickness of the strip on the working side is greater than or equal to the middle thickness of the strip as an example, when the edge thickness of the strip on the working side is greater than or equal to the middle thickness of the strip, when the working roll bending value is adjusted, the upper working roll bending value of the upper working roll 205 needs to be adjusted, and the upper working roll bending value is adjusted multiple times. In each adjustment, the upper working roll bending value is reduced by 0.5 tons until the edge thickness is less than the middle thickness.

[0052] It should be noted here that the bending value of the upper working roll is reduced by 0.5 tons, that is, a force opposite to the rolling force direction is applied to the upper working roll 205 through the working roll bending value adjustment system (in each adjustment, the applied force is 0.5 tons) to reduce the curvature of the middle part of the upper working roll 205 in the direction of the rolling force, so as to reduce the roll gap between the upper working roll 205 and the lower working roll 206, so that the rolling force of the edge of the strip on the working side is increased, and after multiple adjustments, the edge thickness of the strip on the working side is less than the middle thickness of the strip. The production efficiency and strip yield rate of the production line are greatly improved, and the quality and yield rate of the plate shape are guaranteed.

[0053] The following describes an apparatus embodiment of the present application, which can be used to execute the control method for eliminating the yield line defect at the edge of a steel strip in the above-mentioned embodiment of the present application. For details not disclosed in the apparatus embodiment of the present application, please refer to the above-mentioned embodiment of the control method for eliminating the yield line defect at the edge of a steel strip in the present application.

[0054] Figure 3 It is a structural block diagram of a control device for eliminating yield line defects at the edge of a steel strip according to an embodiment of the present application.

[0055] Reference Figure 3 As shown, according to an embodiment of the present application, a control device 300 for eliminating yield line defects at the edge of a steel strip comprises: a detection unit 301, a pre-judgment unit 302, a first adjustment unit 303, and a second adjustment unit 304.

[0056] The detection unit 301 is used to detect the edge thickness of the steel strip in real time based on the strip position of the steel strip during the cold rolling process of the steel strip.

[0057] The judgment unit 302 is used to predict the existence of edge yield line defects in the strip after annealing if it is continuously detected that the edge thickness is greater than the middle thickness of the strip and the number of consecutive strip points exceeds a preset number.

[0058] The first adjustment unit 303 is used to adjust the working roll shifting value of the cold rolling mill so that the edge thickness is smaller than the middle thickness.

[0059] The second adjustment unit 304 is used to adjust the working roll bending value of the cold rolling mill so that the edge thickness is smaller than the middle thickness if the edge thickness is greater than or equal to the middle thickness after the cumulative adjustment value of the working roll shifting value reaches a first preset value.

[0060] Reference Figure 4 , Figure 4 A schematic diagram of the structure of a computer system suitable for implementing an electronic device of an embodiment of the present application is shown.

[0061] like Figure 4 As shown, the computer system 400 includes a central processing unit (CPU) 401, which can perform various appropriate actions and processes according to the program stored in the read-only memory (ROM) 402 or the program loaded from the storage part 408 to the random access memory (RAM) 403, such as executing the method described in the above embodiment. In the RAM 403, various programs and data required for system operation are also stored. The CPU 401, ROM 402 and RAM 403 are connected to each other through a bus 404. An input / output (I / O) interface 405 is also connected to the bus 404.

[0062] The following components are connected to the I / O interface 405: an input section 406 including a keyboard, a mouse, etc.; an output section 407 including a cathode ray tube (CRT), a liquid crystal display (LCD), etc., and a speaker, etc.; a storage section 408 including a hard disk, etc.; and a communication section 409 including a network interface card such as a LAN (Local Area Network) card, a modem, etc. The communication section 409 performs communication processing via a network such as the Internet. A drive 410 is also connected to the I / O interface 405 as needed. A removable medium 411, such as a magnetic disk, an optical disk, a magneto-optical disk, a semiconductor memory, etc., is installed on the drive 410 as needed so that a computer program read therefrom is installed into the storage section 408 as needed.

[0063] In particular, according to an embodiment of the present application, the process described above with reference to the flowchart can be implemented as a computer software program. For example, an embodiment of the present application includes a computer program product, which includes a computer program carried on a computer-readable medium, and the computer program includes a program code for executing the method shown in the flowchart. In such an embodiment, the computer program can be downloaded and installed from a network through a communication section 409, and / or installed from a removable medium 411. When the computer program is executed by a central processing unit (CPU) 401, various functions defined in the system of the present application are executed.

[0064] It should be noted that the computer-readable medium shown in the embodiment of the present application may be a computer-readable signal medium or a computer-readable storage medium or any combination of the above two. The computer-readable storage medium may be, for example, - but not limited to - an electrical, magnetic, optical, electromagnetic, infrared, or semiconductor system, device or device, or any combination of the above. More specific examples of computer-readable storage media may include, but are not limited to: an electrical connection with one or more wires, a portable computer disk, a hard disk, a random access memory (RAM), a read-only memory (ROM), an erasable programmable read-only memory (EPROM), a flash memory, an optical fiber, a portable compact disk read-only memory (CD-ROM), an optical storage device, a magnetic storage device, or any suitable combination of the above. In the present application, a computer-readable storage medium may be any tangible medium containing or storing a program, which may be used by an instruction execution system, device or device or used in combination with it. In the present application, a computer-readable signal medium may include a data signal propagated in a baseband or as part of a carrier wave, wherein a computer-readable program code is carried. Such propagated data signals may take a variety of forms, including but not limited to electromagnetic signals, optical signals, or any suitable combination of the above. Computer-readable signal media may also be any computer-readable medium other than computer-readable storage media, which may send, propagate, or transmit programs for use by or in conjunction with an instruction execution system, apparatus, or device. The program code contained on the computer-readable medium may be transmitted using any appropriate medium, including but not limited to: wireless, wired, etc., or any suitable combination of the above.

[0065] The flowchart and block diagram in the accompanying drawings illustrate the possible architecture, functions and operations of the system, method and computer program product according to various embodiments of the present application. Wherein, each box in the flowchart or block diagram can represent a module, a program segment, or a part of the code, and the above-mentioned module, program segment, or a part of the code contains one or more executable instructions for realizing the specified logical function. It should also be noted that in some alternative implementations, the functions marked in the box can also occur in a different order from the order marked in the accompanying drawings. For example, two boxes represented in succession can actually be executed substantially in parallel, and they can sometimes be executed in the opposite order, depending on the functions involved. It should also be noted that each box in the block diagram or flowchart, and the combination of boxes in the block diagram or flowchart can be implemented with a dedicated hardware-based system that performs a specified function or operation, or can be implemented with a combination of dedicated hardware and computer instructions.

[0066] The units involved in the embodiments described in this application may be implemented by software or hardware, and the units described may also be set in a processor. The names of these units do not, in some cases, constitute limitations on the units themselves.

[0067] According to a typical embodiment of the present application, the present application also proposes a computer-readable storage medium, in which at least one program code is stored. The at least one program code is loaded and executed by a processor to implement the operations performed by the control method for eliminating yield line defects on the edge of strip as described above.

[0068] According to a typical implementation of the present application, the present application also proposes an electronic device, which includes a memory and a processor, wherein the memory stores a computer program, and is characterized in that when the processor executes the computer program, it implements the operations performed by the control method for eliminating yield line defects on the edge of strip as described above.

[0069] It should be noted that, although several modules or units of the equipment for action execution are mentioned in the above detailed description, this division is not mandatory. In fact, according to the embodiments of the present application, the features and functions of two or more modules or units described above can be embodied in one module or unit. On the contrary, the features and functions of one module or unit described above can be further divided into being embodied by multiple modules or units.

[0070] It can be seen from the above technical solution that the present application has at least the following advantages and positive effects:

[0071] Firstly, the solution proposed in the present application can solve the problem of edge yield line defects in cold-rolled strip after annealing. During the cold rolling process of the strip, the present application can control the edge thickness of the strip to be smaller than the middle thickness of the strip, so as to predict in advance whether the strip will have edge yield line defects in the subsequent annealing treatment, and adjust the cold rolling parameters in time to eliminate the edge yield line defects of the strip, ensure the plate shape and quality of the strip, and improve the production efficiency of the production line and the yield rate of the strip.

[0072] Secondly, the solution proposed in this application is adopted, by adding special equipment in the cold rolling production line to perform real-time detection of the edge thickness of the strip, and when the edge profile thickens, an alarm is promptly issued and the rolling parameters of the cold rolling process are adjusted to control the edge thickness of the strip, thereby reducing the internal stress of the edge of the strip and avoiding the occurrence of edge yield line defects after annealing.

[0073] Thirdly, the solution proposed in this application can greatly reduce the scrapping amount of steel strip and the damage amount of equipment, greatly save resources and equipment maintenance funds, and reduce costs.

[0074] Although the present application has been described with reference to several typical embodiments, it should be understood that the terms used are illustrative and exemplary, rather than restrictive. Since the present application can be implemented in a variety of forms without departing from the spirit or essence of the application, it should be understood that the above-mentioned embodiments are not limited to any of the aforementioned details, but should be widely interpreted within the spirit and scope defined by the attached claims, so all changes and modifications falling within the scope of the claims or their equivalents should be covered by the attached claims.

Claims

1. A control method for eliminating yield line defects at the edge of a strip, characterized in that: The method comprises: In the process of cold rolling the steel strip, the edge thickness of the steel strip is detected in real time based on the steel strip point position of the steel strip; If it is continuously detected that the edge thickness is greater than the middle thickness of the strip, and the number of continuous strip points exceeds a preset number, it is predicted that the strip has an edge yield line defect after annealing; Adjusting the working roll shifting value of the cold rolling mill so that the edge thickness is smaller than the middle thickness; If the edge thickness is greater than or equal to the middle thickness after the cumulative adjustment value of the working roll shifting value reaches a first preset value, the working roll bending value of the cold rolling mill is adjusted so that the edge thickness is less than the middle thickness.

2. The method according to claim 1, characterized in that By installing a strip profile detection device on the cold rolling production line, the edge thickness of the strip is detected in real time based on the strip point position of the strip.

3. The method according to claim 1, characterized in that The step of adjusting the working roll shifting value of the cold rolling mill so that the edge thickness is smaller than the middle thickness comprises: The working roll shifting value is adjusted multiple times, and in each adjustment, the working roll shifting value is increased by 3 mm until the edge thickness is less than the middle thickness or the cumulative adjustment value of the working roll shifting value reaches a first preset value.

4. The method according to claim 1, characterized in that: The preset number is 5.

5. The method according to claim 1, characterized in that The first preset value is 15 mm.

6. The method according to claim 1, characterized in that The step of adjusting the bending value of the working roll of the cold rolling mill so that the thickness of the edge portion is smaller than the thickness of the middle portion comprises: The working roll bending value is adjusted multiple times. In each adjustment, the working roll bending value is reduced by 0.5 tons until the edge thickness is less than the middle thickness. The cumulative adjustment value of the working roll bending value is a second preset value.

7. The method according to claim 6, characterized in that The second preset value is 4 tons.

8. A control device for eliminating yield line defects at the edge of a strip, characterized in that: The device comprises: The detection unit is used to detect the edge thickness of the steel strip in real time based on the steel strip point position during the cold rolling process of the steel strip; A prejudgment unit is used to predict that the strip has an edge yield line defect after annealing if it is continuously detected that the edge thickness is greater than the middle thickness of the strip and the number of consecutive strip points exceeds a preset number; The first adjustment unit is used to adjust the working roll shifting value of the cold rolling mill so that the edge thickness is smaller than the middle thickness; The second adjustment unit is used to adjust the working roll bending value of the cold rolling mill so that the edge thickness is smaller than the middle thickness if the edge thickness is greater than or equal to the middle thickness after the cumulative adjustment value of the working roll shifting value reaches a first preset value.

9. A computer-readable storage medium, characterized in that: The computer-readable storage medium stores at least one program code, and the at least one program code is loaded and executed by a processor to implement the operations performed by the method according to any one of claims 1 to 7.

10. An electronic device comprising a memory and a processor, wherein the memory stores a computer program, wherein: When the processor executes the computer program, the processor implements the operations performed by the method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Cooperative control method for controlling edge crease defect and edge thickness of cold-rolled strip steel

    CN103302105A

  • Detection method for strip steel local high point

    CN103920723A

  • Edge-drop control method during rolling process

    CN105436208A

  • Prediction method of edge wave generation after cold rolling of low carbon steel

    CN105803172A

  • Roll bending force setting method aiming at cold continuous rolling strip steel head plate shape defects

    CN114951304A

Cited By

  • Preparation method of cold-rolled fine-punched steel plate

    CN121294806A