Nickel aluminum bronze BAL7-7-2-2 bar forging method

Through the nickel-aluminum bronze BAL7-7-2-2 bar forging method, including mold-assisted round-drawing and forging frequency control, the uneven structure of nickel-aluminum bronze BAL7-7-2-2 bar in the prior art is solved. and the problem of unstable performance, the forging process with high performance and simplified operation is achieved.

CN119016653APending Publication Date: 2024-11-26CHINA SHIPBUILDING INDUSTRY CORPORATION NO725 RESEARCH INSTITUTE
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411331990.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-26

Smart Images

  • Figure CN119016653A_ABST
    Figure CN119016653A_ABST
Patent Text Reader

Abstract

The invention provides a nickel aluminum bronze BAL7-7-2-2 bar forging method. The nickel aluminum bronze BAL7-7-2-2 bar forging method comprises the following steps that S1, blanking is conducted; s2, heating for a first heating number; s3, primary upsetting; s4, primary rounding and drawing-out; s5, heating for a second heating number; s6, secondary rolling and drawing-out; and S7, annealing treatment. And primary rolling and drawing-out and secondary rolling and drawing-out are carried out with the assistance of the mold, rounding is carried out while drawing-out is carried out, operation simplification is facilitated, and steps are saved. And meanwhile, the forging frequency during one-time upsetting is defined, the overheating phenomenon can be better reduced by implementing the corresponding forging frequencies at different stages, and experience operation of different operators during forging is avoided. By the adoption of the forging method, BAL7-7-2-2 bar billets of different specifications with uniform and fuzzy macrostructures and uniform and fine macrostructures can be obtained, the tensile strength Rm of forged bars is larger than or equal to 500 MPa, the yield strength Rp0.2 is larger than or equal to 240 MPa, the ductility A is larger than or equal to 20%, the corrosion fatigue strength under the indoor-temperature artificial seawater condition is larger than or equal to 125 MPa (the cycle index is 107), and the BAL7-7-2-2 bar billets are suitable for being used as marine materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of processing and manufacturing, and in particular to a forging method for a nickel-aluminum bronze BAL7-7-2-2 bar. Background Art

[0002] Nickel aluminum bronze alloy is widely used in ship propellers, large pump impellers, fasteners, seawater valves and filters due to its excellent resistance to stress cracking, corrosion fatigue, cavitation corrosion, erosion and marine biofouling. With the widespread application of nickel aluminum bronze, its use environment has put forward higher requirements on its own mechanical properties and organizational uniformity. Traditional nickel aluminum bronze is generally in a cast state. The typical nickel aluminum bronze cast structure is composed of coarse α particles, various K phases and martensite. In addition, defects such as uneven composition and voids are prone to occur during the alloy casting process. The poor organization makes the tensile strength and yield strength of nickel aluminum bronze castings generally low, and the precipitation inside the alloy presents a granular distribution state.

[0003] Invention patent application CN201510201613.6 A nickel-aluminum bronze alloy and its preparation method introduces a method for preparing a nickel-aluminum bronze alloy raw material with high hardness and high wear resistance by changing the ratio of Mn, Al, Fe, and Ni elements; Invention patent application CN202210514951.5 Nickel-aluminum bronze laser additive manufacturing method introduces a nickel-aluminum bronze laser additive manufacturing method; Invention patent application CN201811592724.4 An ultra-short cycle high-strength-high ductility nickel-aluminum bronze alloy Gold and its preparation method introduces a method of preparing nickel-aluminum bronze alloy powder by plasma electrode atomization, and using selective electron beam melting process to obtain high-density, high-strength and high-ductility nickel-aluminum bronze alloy through 3D printing; Invention patent application CN202210531203.8 A heat treatment process method to improve the strength and toughness of nickel-aluminum bronze alloy introduces a heat treatment process method to improve the strength and toughness of nickel-aluminum bronze (QAL10-4-4, QAL9-4-4, QAL10-6-6, QAL10-5-5) alloy.

[0004] The above patents do not involve the forging method of nickel aluminum bronze BAL7-7-2-2 bars with different specifications and diameters and high mechanical properties and corrosion resistance, and there are few related reports. Although the invention patent application CN202210370948.0, a forging method of marine copper-nickel alloy BFe30-1-1 bars, records the forging method, it is for copper-nickel alloys and the method is relatively complicated. Summary of the invention

[0005] In view of this, the present invention aims to propose a nickel-aluminum bronze BAL7-7-2-2 bar forging method for preparing nickel-aluminum bronze BAL7-7-2-2 bars with uniform structure and stable performance, so as to solve the defect of the prior art that there is no forging process for preparing nickel-aluminum bronze BAL7-7-2-2 bars.

[0006] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0007] A method for forging a nickel-aluminum bronze BAL7-7-2-2 bar comprises the following steps:

[0008] S1. Cutting

[0009] The ingot of nickel aluminum bronze BAL7-7-2-2 is selected as the raw material blank, and the weight required for the finished nickel aluminum bronze BAL7-7-2-2 forging rods of different diameter specifications is used as the reference weight for blanking. The height-to-diameter ratio of the circular cross-section blank should not exceed 3;

[0010] S2. First fire heating

[0011] The nickel aluminum bronze BAL7-7-2-2 billet is heated, and the billet heating temperature is controlled at 950-990°C. During the heating process, the billet is turned over as needed to ensure uniform heating. The final forging temperature of the billet is 800-850°C.

[0012] S3. One-time roughing

[0013] The heated billet is roughened for the first time, and the roughening ratio is controlled between 2.0 and 3.0. During the forging process, the forging frequency is controlled at 110 to 120 times / minute at the beginning, 80 to 100 times / minute in the middle, and 110 to 120 times / minute at the end;

[0014] S4. One-time rounding and lengthening

[0015] For nickel-aluminum bronze BAL7-7-2-2 bars with a diameter not exceeding 65 mm, after the primary roughening is completed, the blank is turned over for transverse drawing, and then the first end is clamped, and the second end is transversely rounded and drawn. The primary rounding and drawing is performed with the assistance of a mold, and the blank is drawn to the corresponding specifications according to the actual situation to obtain a primary cylindrical blank with a cylindrical second end, and the diameter of the second end differs from the diameter of the finished nickel-aluminum bronze BAL7-7-2-2 bar by 10 to 20 mm;

[0016] For nickel-aluminum bronze BAL7-7-2-2 bars with a diameter greater than 65 mm, after the first roughening is completed, the blank is turned over for end face trimming, and the blank is turned over again for longitudinal drawing, and then the first end is clamped, and the second end is rounded and drawn along the longitudinal direction of the blank. The first rounding and drawing is performed with the assistance of a mold, and the blank is drawn to the corresponding specifications according to the actual situation to obtain a primary cylindrical blank with a cylindrical second end, and the diameter of the second end is 10 to 20 mm different from the diameter of the finished nickel-aluminum bronze BAL7-7-2-2 bar;

[0017] S5. Second fire heating

[0018] The primary cylindrical billet obtained in step S4 is subjected to a second heating at a temperature of 980°C ± 10°C and a holding time of 30 to 60 minutes;

[0019] S6. Second rounding and lengthening

[0020] The blank obtained in step S5 is turned over at both ends, the second end is clamped, and the first end is rounded and stretched. The second rounding and stretching process is opposite to the clamping end and the stretching end in the first rounding and stretching process, and the rounding and stretching operation in step S4 is repeated;

[0021] After the secondary tumbling and elongation treatment, the first end of the primary cylindrical blank also becomes cylindrical, and the diameter of the first end differs from the diameter of the finished nickel aluminum bronze BAL7-7-2-2 rod by 10 to 20 mm, so that a regular cylindrical blank is obtained for standby use;

[0022] S7. Annealing

[0023] The obtained regular cylindrical billet is annealed at a temperature of 880°C to 900°C for a holding time of 45 to 90 minutes, and then air-cooled after being taken out of the furnace.

[0024] Furthermore, one end of the blank is recorded as the first end, and the other end is recorded as the second end. When rounding and stretching are performed, it is carried out with the assistance of a mold. The mold has a groove, and the groove is semi-cylindrical. The end of the blank to be processed is placed in the groove, and the press applies pressure to shape the end placed in the groove. After forming, it is rotated 180° and pressure is continued to be applied to shape one end of the blank to form a cylinder.

[0025] Furthermore, in step S4, after the first roughening is completed, the blank is turned over, the first end is clamped, and the second end is transversely rounded and drawn. The first rounding and drawing are carried out with the assistance of a mold, and the blank is drawn to a corresponding specification to obtain a primary cylindrical blank with a cylindrical second end, and the diameter of the second end differs from the diameter of the finished nickel-aluminum bronze BAL7-7-2-2 rod by 10 to 20 mm.

[0026] Furthermore, in step S6, the two ends of the blank obtained in step S5 are turned over, the second end is clamped, and the first end is rounded and stretched with the assistance of a mold. The secondary rounding and stretching treatment is opposite to the clamping end and the stretching end during the primary rounding and stretching treatment. After the secondary rounding and stretching treatment, the diameter of the first end differs from the diameter of the finished nickel-aluminum bronze BAL7-7-2-2 rod by 10 to 20 mm, and a regular cylindrical blank is obtained.

[0027] Further, in step S1, the blanking weight M of the nickel aluminum bronze BAL7-7-2-2 forging rod not larger than Φ65 mm 下 =M 锻 ×1.02, where M 锻 The weight of the finished nickel-aluminum bronze BAL7-7-2-2 forged rod; the blank weight M of the nickel-aluminum bronze BAL7-7-2-2 forged rod with a diameter greater than Φ65mm 下 =M 锻 ×1.03, where M 锻 The weight of the finished nickel aluminum bronze BAL7-7-2-2 forged bar.

[0028] Furthermore, in step S2, an electric furnace is used to heat the nickel aluminum bronze BAL7-7-2-2 billet, and the billet is heated by charging the furnace when it reaches a certain temperature or heating the billet along with the furnace.

[0029] Furthermore, in step S3, when the forging time is 3 minutes, the initial stage is 0.5±0.2 minutes, the middle stage is 2±0.2 minutes, and the final stage is 0.5±0.2 minutes.

[0030] Compared with the prior art, the nickel aluminum bronze BAL7-7-2-2 bar forging method described in the present invention has the following advantages:

[0031] 1. With the help of the mold, the first rounding and stretching and the second rounding and stretching are carried out, and rounding is carried out while stretching, which is conducive to simplifying the operation and saving steps;

[0032] 2. The forging frequency during a roughing process is clarified. By implementing the corresponding forging frequency at different stages, overheating can be better reduced, and the experience of different operators during forging can be avoided;

[0033] 3. By forging the ingot of nickel aluminum bronze BAL7-7-2-2, the blank is fully plastically deformed, which is conducive to eliminating the defects of the internal structure. Through a series of roughening and drawing, the structure of the rod billet is more uniform. By controlling the deformation mode of the rod billet of different specifications, the grains of the rod billet are fully broken. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0035] Figure 1 It is a structural schematic diagram of the mold described in the present invention.

[0036] Description of reference numerals:

[0037] 1. Mold; 2. Groove; DETAILED DESCRIPTION

[0038] The present invention will be further described below in conjunction with specific embodiments. It should be noted that the data in the following experimental examples are obtained by the inventor through a large number of experiments. Due to space limitations, only a part of them is shown in the specification, and those of ordinary skill in the art can understand and implement the present invention under these data. These embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these changes or modifications also fall within the scope protected by the present application.

[0039] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0040] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.

[0041] The present invention provides a nickel aluminum bronze BAL7-7-2-2 bar forging method, which specifically comprises the following steps:

[0042] S1. Cutting

[0043] The ingot of nickel aluminum bronze BAL7-7-2-2 is selected as the raw material blank, and the weight required for the finished nickel aluminum bronze BAL7-7-2-2 forging rods of different diameter specifications is used as the reference weight for blanking. The height-to-diameter ratio of the circular cross-section blank should not exceed 3;

[0044] Nickel aluminum bronze BAL7-7-2-2 forging rod with a diameter not exceeding Φ65mm 下 =M 锻 ×1.02, where M 锻 The weight of the finished nickel-aluminum bronze BAL7-7-2-2 forged rod. That is, for nickel-aluminum bronze BAL7-7-2-2 forged rods with a diameter not exceeding Φ65mm, the blank weight is the weight of the finished forged rod plus 2% of the burn loss.

[0045] Nickel aluminum bronze BAL7-7-2-2 forging rod with diameter greater than Φ65mm 下 =M锻 ×1.03, where M 锻 The weight of the finished nickel aluminum bronze BAL7-7-2-2 forged rod. That is, for nickel aluminum bronze BAL7-7-2-2 forged rods with a diameter greater than Φ65mm, the blank weight is the weight of the finished forged rod plus 3% of the burn loss.

[0046] In order to reduce the loss of cutting materials, a laser cutting machine is selected to saw and cut materials according to the specifications of the finished forged bars. The laser cutting machine has the advantages of high precision and low loss.

[0047] S2. First fire heating

[0048] The nickel aluminum bronze BAL7-7-2-2 billet is heated, and the billet heating temperature is controlled at 950-990°C. During the heating process, the billet is turned over as needed to ensure uniform heating. The final forging temperature of the billet is 800-850°C.

[0049] Specifically, an electric furnace is used to heat the nickel aluminum bronze BAL7-7-2-2 billet, and the billet is heated by charging the furnace at a certain temperature or heating it with the furnace. When charging the furnace at a certain temperature, the billet is kept warm for no less than 3 hours, and when the hot material is returned to the furnace, the holding time is halved; when heating it with the furnace, the billet is kept warm for no less than 1.5 hours.

[0050] S3. One-time roughing

[0051] The heated billet is axially upset for the first time, and the upset ratio is controlled between 2.0 and 3.0. During the forging process, the forging frequency is controlled at 110 to 120 times / minute at the beginning, 80 to 100 times / minute in the middle, and 110 to 120 times / minute at the end;

[0052] Specifically, in order to prevent the end from folding during the subsequent drawing process, the first upsetting ratio is controlled between 2.0 and 3.0. During forging, heavy hammer hitting quickly can easily cause local thermal effects and thus overheating. Therefore, the present invention adopts a forging frequency of 110 to 120 times / minute in the initial stage, 80 to 100 times / minute in the middle stage, and 110 to 120 times / minute in the final stage to avoid continuous fast hammer hitting, better reduce overheating, and ensure uniform forging deformation. At the same time, since the forging frequency is fixed, the experience operation of different operators during forging is avoided, reducing errors.

[0053] More specifically, the initial stage, the middle stage and the final stage are determined based on empirical values. Generally, if the forging time is 3 minutes, the initial stage is 0.5±0.2 minutes, the middle stage is 2±0.2 minutes, and the final stage is 0.5±0.2 minutes.

[0054] S4. One-time rounding and lengthening

[0055] For the convenience of description, one end of the blank is recorded as the first end, and the other end is recorded as the second end.

[0056] The rounding and stretching is carried out with the assistance of a mold 1, wherein the mold 1 has a groove 2, and the groove 2 is semi-cylindrical. The mold 1 extends along the axial direction of the groove 2 to form a certain length, which is convenient for placing the blank. The extension length can be set by the operator according to the empirical value. When in use, the end of the blank to be processed is placed in the groove 2, and the press applies pressure to shape the end placed in the groove 2. After forming, it is rotated 180° and continues to apply pressure to shape one end of the blank into a cylindrical shape. Since the rounding and stretching of the blank is carried out in the groove 2, a columnar blank can be directly obtained.

[0057] For a nickel-aluminum bronze BAL7-7-2-2 bar with a diameter not greater than 65 mm, after the primary roughening is completed, the blank is turned over for transverse stretching, and then the first end is clamped, and the second end is transversely rounded and stretched. The primary rounding and stretching is performed with the assistance of a mold 1. The blank is stretched to a corresponding specification according to actual conditions to obtain a primary cylindrical blank with a cylindrical second end, and the diameter of the second end differs from the diameter of the finished nickel-aluminum bronze BAL7-7-2-2 bar by 10 to 20 mm.

[0058] For nickel-aluminum bronze BAL7-7-2-2 bars with a diameter greater than 65 mm, after the first roughening is completed, the blank is turned over for end face trimming, and the blank is turned over again for longitudinal drawing. Then, the first end is clamped, and the second end is rounded and drawn along the longitudinal direction of the blank. The first rounding and drawing is carried out with the assistance of mold 1. According to the actual situation, it is drawn to the corresponding specifications to obtain a primary cylindrical blank with a cylindrical second end, and the diameter of the second end differs by 10 to 20 mm from the diameter of the finished nickel-aluminum bronze BAL7-7-2-2 bar.

[0059] The transverse direction mentioned in the present application refers to the axial direction of forming a cylindrical blank, and the longitudinal direction mentioned in the present application refers to the axial direction perpendicular to the cylindrical blank, that is, the diameter direction.

[0060] Diagonal cracks should be avoided on the end face of the billet during rounding and drawing. The feed amount during drawing should be 0.3-0.7 of the anvil width, the forging ratio should not be less than 3, and the final forging temperature should be 800-850℃.

[0061] In the prior art, this step is to square the drawn end, and the drawn end is deformed into a square after the square drawing. In order to obtain the finished forged rod, the obtained regular square billet needs to be rounded and shaped. However, in the present invention, in the rounding and drawing step, with the assistance of the die 1, the primary cylindrical billet can be obtained after the rounding and drawing, avoiding the rounding and shaping in the subsequent process, simplifying the steps and saving time.

[0062] S5. Second fire heating

[0063] The primary cylindrical billet obtained in step S4 is subjected to a second heating at a temperature of 980°C ± 10°C and a heat preservation time of 30 to 60 minutes.

[0064] S6. Second rounding and lengthening

[0065] The blank obtained in step S5 is turned at both ends, the second end is clamped, and the first end is rounded and stretched with the assistance of the mold 1. The second rounding and stretching process is opposite to the clamping end and the stretching end in the first rounding and stretching process, and the rounding and stretching operation in step S4 is repeated;

[0066] After the secondary tumbling and stretching treatment, the first end of the primary cylindrical billet also becomes cylindrical, and the diameter of the first end differs from the diameter of the finished nickel-aluminum bronze BAL7-7-2-2 rod by 10 to 20 mm, thereby obtaining a regular cylindrical billet for use.

[0067] S7. Annealing

[0068] The obtained regular cylindrical billet is annealed at a temperature of 880°C to 900°C for a holding time of 45 to 90 minutes, air-cooled after being taken out of the furnace, and a blank bar is obtained, which is then machined to obtain a finished forged bar.

[0069] Specifically, the annealing treatment is carried out in a warm charging furnace. The annealing treatment can eliminate the internal stress and make the grain structure of the rod blank uniform. After the heat treatment, the structure is α matrix + dispersed precipitate phase.

[0070] The nickel aluminum bronze BAL7-7-2-2 bar forging method of the present invention can obtain BAL7-7-2-2 bar blanks of different specifications with uniform and fuzzy low-magnification structure and uniform and fine high-magnification structure, and the forged bar has a tensile strength Rm≥500MPa, a yield strength Rp0.2≥240MPa, an elongation A≥20%, and a corrosion fatigue strength of ≥125MPa (cycle number 10 under room temperature artificial seawater conditions). 7 ), suitable as ship material.

[0071] The nickel aluminum bronze BAL7-7-2-2 bar forging method of the present invention has the following advantages:

[0072] 1. With the assistance of mold 1, the first rounding and stretching and the second rounding and stretching are performed, and rounding is performed while stretching, which is conducive to simplifying the operation and saving steps;

[0073] 2. The forging frequency during a roughing process is clarified. By implementing the corresponding forging frequency at different stages, overheating can be better reduced, and the experience of different operators during forging can be avoided;

[0074] 3. By forging the ingot of nickel aluminum bronze BAL7-7-2-2, the blank is fully plastically deformed, which is conducive to eliminating the defects of the internal structure. Through a series of roughening and drawing, the structure of the rod billet is more uniform. By controlling the deformation mode of the rod billet of different specifications, the grains of the rod billet are fully broken.

[0075] Example 1 Production of Φ65mm×1000mm Nickel Aluminum Bronze BAL7-7-2-2 Rods

[0076] The specific production process is as follows: According to the bar specifications required for the finished product, the weight of a single piece of material is approximately 39.3kg, the forging blanking weight is the material weight plus 2% forging burn loss, the final blanking weight is approximately 40.1kg, and the blanking specifications are Φ280mm×80mm.

[0077] The blank is heated for the first time at a temperature of 980°C ± 10°C for 3 hours.

[0078] After the first heating, the blank is subjected to a roughing deformation to Φ285mm×76mm. During the roughing process, the forging frequency is controlled at 120 times / minute at the beginning, 100 times / minute in the middle, and 110 times / minute at the end.

[0079] After the roughening deformation, the blank is turned over and stretched horizontally to Φ140mm×315mm. The jaws clamp the first end, and with the assistance of the mold 1, the second end of the blank is placed in the groove 2. The press applies pressure to cyclically deform the second end of the blank, round it horizontally and stretch it to a second end diameter of 75mm, to obtain a primary cylindrical blank with a second end diameter close to that of the finished nickel aluminum bronze BAL7-7-2-2 bar.

[0080] The obtained primary cylindrical billet is subjected to a second heating at a temperature of 980°C ± 10°C and a holding time of 30 minutes.

[0081] After the second round of heating is completed and the blank is taken out of the furnace, the clamping end of the blank is turned, and the second end that has been rounded and stretched is clamped with jaws. The same rounding and stretching operation is performed on the first end until the diameter of the first end is 75mm. The diameter of the first end is close to the diameter of the finished nickel-aluminum bronze BAL7-7-2-2 rod, and a regular cylindrical blank is obtained.

[0082] The obtained regular cylindrical billet is annealed by a warm-charging furnace, the annealing temperature is 890℃±10℃, the holding time is 60 minutes, and the billet is air-cooled after being taken out of the furnace. After machining, a nickel-aluminum bronze BAL7-7-2-2 finished forged bar of Φ65mm×1000mm is obtained.

[0083] Example 2 Production of Φ180mm×1000mm Nickel Aluminum Bronze BAL7-7-2-2 Rods

[0084] The specific production process is as follows: According to the bar specifications required for the finished product, the weight of a single piece of material is approximately 261kg, the forging blanking weight is the material weight plus 3% forging burn loss, the final blanking weight is approximately 268.8kg, and the blanking specifications are Φ281mm×497mm.

[0085] The blank is heated for the first time at a temperature of 980°C ± 10°C for 3 hours.

[0086] After the first heating, the blank is subjected to a roughing deformation to Φ363mm×297mm. During the roughing process, the forging frequency is controlled at 110 times / minute at the beginning, 80 times / minute in the middle, and 120 times / minute at the end.

[0087] After the deformation, the direction is turned and the longitudinal length is stretched to Φ300×433mm, and the direction is turned again and the longitudinal length is stretched to Φ250×625mm to ensure sufficient deformation in the case of larger diameter. The jaws clamp the first end, and with the assistance of the mold 1, the second end of the blank is placed in the groove 2. The press applies pressure to round and stretch the second end of the blank along the longitudinal direction of the blank to a second end diameter of 190mm, and obtain a primary cylindrical blank with a second end diameter close to the diameter of the finished nickel aluminum bronze BAL7-7-2-2 bar.

[0088] The obtained primary cylindrical billet is subjected to a second heating at a temperature of 980°C ± 10°C and a holding time of 1 hour.

[0089] After the second round of heating is completed and the blank is taken out of the furnace, the clamping end of the blank is turned, and the second end that has been rounded and stretched is clamped with jaws. The same rounding and stretching operation is performed on the first end until the diameter of the first end is 190 mm. The diameter of the first end is close to the diameter of the finished nickel-aluminum bronze BAL7-7-2-2 bar, and a regular cylindrical blank is obtained.

[0090] The obtained regular cylindrical billet is annealed by a warm-charging furnace, the annealing temperature is 890℃±10℃, the holding time is 80 minutes, and the billet is air-cooled after being taken out of the furnace to obtain a blank bar. After machining, a nickel-aluminum bronze BAL7-7-2-2 finished forged bar of Φ180mm×1000mm is obtained.

[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for forging nickel aluminum bronze BAL7-7-2-2 bars, It is characterized in that The steps include: S1. Cutting The ingot of nickel aluminum bronze BAL7-7-2-2 is selected as the raw material blank, and the weight required for the finished nickel aluminum bronze BAL7-7-2-2 forging rods of different diameter specifications is used as the reference weight for blanking. The height-to-diameter ratio of the circular cross-section blank should not exceed 3; S2. First fire heating The nickel aluminum bronze BAL7-7-2-2 billet is heated, and the billet heating temperature is controlled at 950-990°C. During the heating process, the billet is turned over as needed to ensure uniform heating. The final forging temperature of the billet is 800-850°C. S3. One-time roughing The heated billet is roughened for the first time, and the roughening ratio is controlled between 2.0 and 3.

0. During the forging process, the forging frequency is controlled at 110 to 120 times / minute at the beginning, 80 to 100 times / minute in the middle, and 110 to 120 times / minute at the end; S4. One-time rounding and lengthening For a nickel-aluminum bronze BAL7-7-2-2 bar with a diameter not greater than 65 mm, after the primary roughening is completed, the blank is turned over and stretched horizontally, and then the first end is clamped and the second end is horizontally rounded and stretched. The primary rounding and stretching is performed with the assistance of a mold (1). The blank is stretched to a corresponding specification according to actual conditions to obtain a primary cylindrical blank with a cylindrical second end, and the diameter of the second end differs from the diameter of the finished nickel-aluminum bronze BAL7-7-2-2 bar by 10 to 20 mm. For a nickel-aluminum bronze BAL7-7-2-2 bar with a diameter greater than 65 mm, after the first roughening is completed, the blank is turned over to trim the end surface, and the blank is turned over again to be longitudinally stretched, and then the first end is clamped, and the second end is rounded and stretched along the longitudinal direction of the blank. The first rounding and stretching is performed with the assistance of a mold (1), and the blank is stretched to a corresponding specification according to actual conditions to obtain a primary cylindrical blank with a cylindrical second end, and the diameter of the second end differs from the diameter of the finished nickel-aluminum bronze BAL7-7-2-2 bar by 10 to 20 mm; S5. Second fire heating The primary cylindrical billet obtained in step S4 is subjected to a second heating at a temperature of 980°C ± 10°C and a holding time of 30 to 60 minutes; S6. Second rounding and lengthening The blank obtained in step S5 is turned over at both ends, the second end is clamped, and the first end is rounded and stretched. The second rounding and stretching process is opposite to the clamping end and the stretching end in the first rounding and stretching process, and the rounding and stretching operation in step S4 is repeated; After the secondary tumbling and elongation treatment, the first end of the primary cylindrical blank also becomes cylindrical, and the diameter of the first end differs from the diameter of the finished nickel aluminum bronze BAL7-7-2-2 rod by 10 to 20 mm, so that a regular cylindrical blank is obtained for standby use; S7. Annealing The obtained regular cylindrical billet is annealed at a temperature of 880°C to 900°C for a holding time of 45 to 90 minutes, and then air-cooled after being taken out of the furnace.

2. The method for forging a nickel aluminum bronze BAL7-7-2-2 bar according to claim 1, It is characterized in that One end of the blank is recorded as the first end, and the other end is recorded as the second end. When rounding and stretching are performed, it is performed with the assistance of a mold (1). The mold (1) has a groove (2), and the groove (2) is semi-cylindrical. The end of the blank to be processed is placed in the groove (2), and a press applies pressure to shape the end placed in the groove (2). After forming, it is rotated 180 degrees and pressure is continued to be applied to shape the end of the blank to form a cylinder.

3. The method for forging a nickel aluminum bronze BAL7-7-2-2 bar according to claim 2, It is characterized in that In step S4, after the primary roughening is completed, the blank is turned over, the first end is clamped, and the second end is transversely rounded and drawn. The primary rounding and drawing is carried out with the assistance of the mold (1), and the blank is drawn to the corresponding specifications to obtain a primary cylindrical blank with a cylindrical second end, and the diameter of the second end is 10 to 20 mm different from the diameter of the finished nickel aluminum bronze BAL7-7-2-2 rod.

4. The method for forging a nickel aluminum bronze BAL7-7-2-2 bar according to claim 2, It is characterized in that In step S6, the two ends of the blank obtained in step S5 are turned over, the second end is clamped, and the first end is rounded and stretched with the assistance of the mold (1). The second rounding and stretching treatment is opposite to the clamping end and the stretching end in the first rounding and stretching treatment. After the second rounding and stretching treatment, the diameter of the first end is 10 to 20 mm different from the diameter of the finished nickel aluminum bronze BAL7-7-2-2 rod, so that a regular cylindrical blank is obtained.

5. The method for forging a nickel aluminum bronze BAL7-7-2-2 bar according to claim 1, It is characterized in that In step S1, the blanking weight M of the nickel aluminum bronze BAL7-7-2-2 forging rod not larger than Φ65 mm 下 =M 锻 ×1.02, where M 锻 The weight of the finished nickel-aluminum bronze BAL7-7-2-2 forged rod; the blank weight M of the nickel-aluminum bronze BAL7-7-2-2 forged rod with a diameter greater than Φ65mm 下 =M 锻 ×1.03, where M 锻 The weight of the finished nickel aluminum bronze BAL7-7-2-2 forged bar.

6. The method for forging a nickel aluminum bronze BAL7-7-2-2 bar according to claim 1, It is characterized in that In step S2, an electric furnace is used to heat the nickel aluminum bronze BAL7-7-2-2 blank, and the blank is heated by charging the furnace when it reaches temperature or heating it with the furnace.

7. The method for forging a nickel aluminum bronze BAL7-7-2-2 bar according to claim 1, It is characterized in that In step S3, when the forging time is 3 minutes, the initial stage is 0.5±0.2 minutes, the middle stage is 2±0.2 minutes, and the final stage is 0.5±0.2 minutes.

Citation Information

Patent Citations

  • Preparation method for ZQA19-4-4-2 nickel aluminum bronze alloy tubes and bars

    CN107794403A

  • Preparation method of copper alloy with good ductility

    CN112267045A

  • Forging method of marine copper-nickel alloy BFe30-1-1 bar

    CN114850364A

  • Manufacture of copper alloy casting

    JP1986023754A