Double-alloy turbine disc laser additive manufacturing method and heat conduction device

Through the combination of laser additive manufacturing and thermal conductivity devices, the defects of traditional welding processes under high temperature and high pressure conditions are solved, and the high-performance manufacturing of dual alloy turbine discs is realized, which reduces the manufacturing cost and cycle. It is suitable for lasers of high-temperature alloy materials. Additive manufacturing.

CN119016746APending Publication Date: 2024-11-26HANGFA EXCELLENT MATERIALS (ZHENJIANG) ADDITIVE MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411078552.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The welding process of traditional dual alloy turbine discs is prone to defects under high temperature and high pressure conditions, affecting the stability and safety of the engine, and is difficult to meet the performance improvement needs of aircraft engines.

Method used

The laser additive manufacturing method is used to combine thermal conductivity devices to manufacture dual alloy turbine disks through laser deposition forming and thermal isostatic pressure + solid solution dual aging treatment to avoid welding defects and improve manufacturing accuracy and reliability.

Benefits of technology

It realizes high-performance manufacturing of dual alloy turbine discs, reduces manufacturing costs and cycles, improves the performance of parts, and is suitable for laser additive manufacturing of high-temperature alloy materials, solving the problems of easy cracking and difficult forming.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016746A_ABST
    Figure CN119016746A_ABST
Patent Text Reader

Abstract

The invention discloses a double-alloy turbine disc laser additive manufacturing method and a heat conduction device, the double-alloy turbine disc laser additive manufacturing device comprises a pair of rotating bodies capable of synchronously rotating along with a turbine disc body, and cooling airflow channels are formed in the edges of one ends of the rotating bodies; the method comprises the steps that firstly, a to-be-subjected-to-additive-manufacturing blade area of a turbine disc body formed through selective laser melting is subjected to primary polishing; 2, performing fluorescence detection on the to-be-processed area, wherein no fluorescence is displayed in the processing area; the part is cleaned and dried through an ultrasonic cleaning machine, and the center line of the to-be-machined face in the thickness direction is marked; according to the powder feeding laser additive manufacturing method, manufacturing of the double-alloy turbine disc is successfully achieved, parts are qualified through fluorescence and X-ray detection, and the manufactured parts have good use performance; the method is not only suitable for laser additive manufacturing of the double-alloy turbine disc, but also can be popularized to similar high-temperature alloy materials and structures which are easy to crack and difficult to form.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of turbine disk processing, and in particular relates to a laser additive manufacturing method for a double-alloy turbine disk and a heat conduction device. Background Art

[0002] The turbine disc is one of the main parts of aircraft engines. As a key part of aircraft engines, it is subjected to the superposition of high temperature and high stress, and has extremely harsh working conditions, complex manufacturing processes, and high technical difficulty. It has long been one of the difficulties in the development of my country's engines. With the continuous improvement of the requirements for aircraft engines, the core components of aircraft engines made of a single alloy can no longer meet the performance requirements. The use of dual-alloy turbine discs that can simultaneously meet different mechanical performance requirements has become an inevitable trend.

[0003] Traditional dual alloy turbine disks are made by diffusion welding the disk body and the blade ring. Since such disks are high-speed rotating parts and work under extreme conditions such as high load, high temperature, and high pressure for a long time, defects in the welding area will directly affect the stability and safety of the engine. In order to better manufacture dual alloy turbine disks with excellent performance, the present invention proposes a method for laser additive manufacturing of dual alloy turbine disks. This method has a short production cycle, high feasibility, and lower manufacturing difficulty. In terms of joint performance, this method is superior to diffusion welding and is not prone to welding defects, and can be better applied to extreme working conditions of turbine disks. Summary of the invention

[0004] The object of the present invention is to provide a laser additive manufacturing method for a dual alloy turbine disk and a heat conducting device to solve the problems raised in the above background technology.

[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solutions: a heat conduction device for laser additive manufacturing of a dual-alloy turbine disk, comprising a pair of rotating bodies that can rotate synchronously with the turbine disk body, a cooling air flow channel is provided at one end edge of the pair of rotating bodies, a stationary body that is stationary relative to the rotating body is provided on the cooling air flow channel, the stationary body is composed of two semicircular rings to form a closed circular ring structure, and the joint of the two semicircular rings is fixedly connected by a fixing piece, a positioning protrusion for limiting is provided on the inner side of the stationary body corresponding to the cooling air flow channel, each of the stationary bodies is provided with a pair of connecting ports, and the connecting ports are connected to the corresponding cooling air flow channels, and a plurality of fastening nuts A for fixing the rotating body to the turbine disk body are provided on the rotating body.

[0006] Preferably, the fixing member includes a gasket located at the joint of the two semicircular rings, and both ends of the gasket are fixedly connected to the two semicircular rings by fastening nuts B respectively.

[0007] Preferably, the rotating body is made of copper and has a through-type structure.

[0008] Preferably, the positioning protrusion only extends to one third of the depth in the cooling air flow channel.

[0009] A method for laser additive manufacturing of a dual alloy turbine disk, using the heat conducting device, specifically comprising the following steps: Step 1: performing initial polishing on the blade area to be additively manufactured of the turbine disk body formed by laser selective melting; removing the surface oxide film by mechanical processing and ensuring that the concentricity between the surface to be processed and the clamping end is not greater than 0.1 mm;

[0010] Step 2: Perform fluorescence detection on the processing area, and there is no fluorescence display in the processing area; use an ultrasonic cleaning machine to clean and dry the parts, and mark the center line of the thickness direction of the processing surface;

[0011] Step 3: Use 3D modeling software to process the blade model, and import it into 3dAMPPPlanner software to generate a printing trajectory and output the printing trajectory file layer by layer;

[0012] Step 4: Install the heat conduction device of the disk body. First, insert a pair of rotating body sets into the corresponding parts of the disk body and fix them with fastening nut A to ensure that they fit tightly with the disk body to prevent slippage when the disk body rotates; then assemble the two semicircular rings that make up the stationary body to the corresponding rotating body, and then splice them with fastening nut B and gaskets; finally, install the inlet pipe and outlet pipe on a pair of connecting ports on the same stationary body respectively; after the cooling tooling is installed, fix the parts on the processing table and adjust the coaxiality of the part processing surface to be less than 0.2mm;

[0013] Step 5: Take an appropriate amount of K477 powder with a particle size of 15 to 53 μm, dry the powder in an oven, and then pour it into the powder feeding device;

[0014] Step 6: Use a fully enclosed inert gas protected laser direct deposition forming equipment to print the blade; after each layer of the blade is printed, wait for the substrate to cool down to below 50°C before printing the next layer;

[0015] Step 7: Perform hot isostatic pressing + solid solution double aging treatment on the turbine disc after printing;

[0016] Step 8: Process the dual alloy turbine disc blank into the required size according to the drawing.

[0017] Preferably, in step five, the particle size of K477 powder is 15-53 μm, the oven baking temperature is 100° C., and the baking time is 1 hour.

[0018] Preferably, the process parameters of step six are as follows: laser power 400-600 W, powder feeding amount 2.5-3 g / min, overlap rate 50%, filling scanning speed 650-750 mm / min, contour scanning speed 400-500 mm / min, powder feeding gas flow rate 8-10 L / min, shielding gas flow rate 20-25 L / min, the angle between the high-pressure turbine disk scanning trajectory and the positive direction of the X-axis is +20°-+30°, the angle between the low-pressure turbine disk scanning trajectory and the positive direction of the X-axis is -60--70°, the number of offset contours is 1-3, the scanning trajectory is a parallel line + contour offset, and the starting point is exchanged layer by layer.

[0019] Preferably, in step seven, the hot isostatic pressing system is: temperature 1150-1180°C, pressure 140-180 MPa, and holding time 2-5 h; solid solution double aging system: solid solution at 980°C, holding for 1 h, then rapidly cooling to room temperature with argon, double aging at 720°C, holding for 8 h, cooling to 620°C at 50°C / h, and then rapidly cooling to below 200°C with argon after holding for 8 h before taking out of the furnace.

[0020] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention successfully realizes the manufacturing of dual alloy turbine disks by using the powder feeding laser additive manufacturing method, the parts are qualified after fluorescence and X-ray detection, and the manufactured parts have good performance. The forming process and crack control method of the present invention for K477 are not only applicable to the laser additive manufacturing of the dual alloy turbine disk, but can also be extended to similar high temperature alloy materials and structures that are easy to crack and difficult to form, providing a good solution to the difficulties in laser additive manufacturing of aerospace high temperature alloy materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic structural diagram of the heat conducting device of the present invention;

[0022] Figure 2 It is a schematic diagram of the partial structure of the heat conducting device of the present invention;

[0023] Figure 3 It is a schematic diagram of the structure in which the heat conducting device of the present invention is installed on a disk body;

[0024] In the figure: 1. rotating body; 2. stationary body; 3. fastening nut A; 4. connecting port; 5. gasket; 6. fastening nut B; 7. cooling air flow channel; 8. positioning protrusion. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] See also Figures 1 to 3 , provides a technical solution: a heat conduction device for laser additive manufacturing of a double alloy turbine disk, comprising a pair of rotating bodies 1 that can rotate synchronously with the turbine disk body, a cooling air flow channel 7 is provided at one end edge of the pair of rotating bodies 1, a stationary body 2 that is stationary relative to the rotating body 1 is provided on the cooling air flow channel 7, the stationary body 2 is composed of two semicircular rings to form a closed circular ring structure, and the joint of the two semicircular rings is fixedly connected by a fixing piece, a positioning protrusion 8 for limiting is provided on the inner side of the stationary body 2 corresponding to the cooling air flow channel 7, each stationary body 2 is provided with a pair of connecting ports 4, and the connecting ports 4 are connected with the corresponding cooling air flow channels 7, and a plurality of fastening nuts A3 for fixedly connecting the rotating body 1 to the turbine disk body are provided on the rotating body 1.

[0027] In this embodiment, preferably, the fixing member includes a gasket 5 located at the joint of the two semicircular rings, and both ends of the gasket 5 are fixedly connected to the two semicircular rings through fastening nuts B6.

[0028] In this embodiment, preferably, the rotating body 1 is made of copper, and the rotating body 1 is a through-type structure.

[0029] In this embodiment, preferably, the positioning protrusion 8 only extends to a third of the depth of the cooling air flow channel 7 .

[0030] A method for laser additive manufacturing of a dual alloy turbine disk, using a heat conducting device, specifically comprising the following steps: Step 1: performing initial polishing on the blade area to be additively manufactured of a GH4169 turbine disk body formed by laser selective melting; removing the surface oxide film by mechanical processing and ensuring that the concentricity between the surface to be processed and the clamping end is not greater than 0.1 mm;

[0031] Step 2: Perform fluorescence detection on the processing area, and there is no fluorescence display in the processing area; use an ultrasonic cleaning machine to clean and dry the parts, and mark the center line of the thickness direction of the processing surface;

[0032] Step 3: Use 3D modeling software to process the blade model, and import it into 3dAMPPPlanner software to generate a printing trajectory and output the printing trajectory file layer by layer;

[0033] Step 4: Install the heat conduction device of the disk body. First, insert a pair of rotating bodies 1 into the corresponding parts of the disk body and fix them with fastening nuts A3 to ensure that they fit tightly with the disk body to prevent slippage when the disk body rotates; then assemble the two semicircular rings that make up the stationary body 2 onto the corresponding rotating body 1, and then splice them with fastening nuts B6 and gaskets 5; finally, install the inlet pipe and the outlet pipe on a pair of connecting ports 4 located on the same stationary body 2 respectively; after the cooling tooling is installed, fix the parts on the processing table and adjust the coaxiality of the part processing surface to be less than 0.2mm;

[0034] Step 5: Take an appropriate amount of K477 powder with a particle size of 15 to 53 μm, dry the powder in an oven, and then pour it into the powder feeding device;

[0035] Step 6: Use a fully enclosed inert gas protected laser direct deposition forming equipment to print the blade; after each layer of the blade is printed, wait for the substrate to cool down to below 50°C before printing the next layer;

[0036] Step 7: Perform hot isostatic pressing + solid solution double aging treatment on the turbine disc after printing;

[0037] Step 8: Process the dual alloy turbine disc blank into the required size according to the drawing.

[0038] In this embodiment, preferably, in step five, the particle size of K477 powder is 15-53 μm, the oven baking temperature is 100° C., and the baking time is 1 hour.

[0039] In this embodiment, preferably, the process parameters of step six are as follows: laser power 400-600W, powder feeding amount 2.5-3g / min, overlap rate 50%, filling scanning speed 650-750mm / min, contour scanning speed 400-500mm / min, powder feeding gas flow rate 8-10L / min, shielding gas flow rate 20-25L / min, the angle between the high-pressure turbine disk scanning trajectory and the positive direction of the X-axis is +20°~+30°, the angle between the low-pressure turbine disk scanning trajectory and the positive direction of the X-axis is -60~-70°, the number of offset contours is 1-3, the scanning trajectory is a parallel line + contour offset, and the starting point is exchanged layer by layer.

[0040] In this embodiment, preferably, in step seven, the hot isostatic pressing system is: temperature 1150-1180°C, pressure 140-180MPa, and holding time 2-5h; solid solution double aging system: solid solution at 980°C, holding for 1h, then rapidly cooling to room temperature with argon, double aging at 720°C, holding for 8h, cooling to 620°C at 50°C / h, and then rapidly cooling to below 200°C with argon after holding for 8h before being taken out of the furnace;

[0041] Turbine disc high temperature durability performance test results table

[0042]

[0043] The device and process of the present invention solve the problems of easy cracking and difficulty in forming a blade with a small wall thickness and a large torsion angle during the K477 additive manufacturing process.

[0044] The turbine disk formed by dual alloy manufacturing has excellent performance and has passed the part-level super-speed and low-cycle fatigue tests. Compared with traditional manufacturing processes, this process greatly reduces the manufacturing cost and cycle of the turbine disk.

[0045] Although embodiments of the present invention have been shown and described (see the above detailed description for details), it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A heat conduction device for laser additive manufacturing of dual alloy turbine disks, characterized in that: The invention comprises a pair of rotating bodies (1) which can rotate synchronously with a turbine disk body, a cooling air flow channel (7) is provided at one end edge of the pair of rotating bodies (1), a stationary body (2) which is stationary relative to the rotating body (1) is provided on the cooling air flow channel (7), the stationary body (2) is composed of two semicircular rings to form a closed circular ring structure, and the joint of the two semicircular rings is fixedly connected by a fixing piece, a positioning protrusion (8) for limiting is provided at the inner side of the stationary body (2) corresponding to the cooling air flow channel (7), each of the stationary bodies (2) is provided with a pair of connecting ports (4), and the connecting ports (4) are connected with the corresponding cooling air flow channel (7), and a plurality of fastening nuts A (3) for fixedly connecting the rotating body (1) to the turbine disk body are provided on the rotating body (1).

2. A heat conduction device for laser additive manufacturing of a dual alloy turbine disk according to claim 1, characterized in that: The fixing member comprises a gasket (5) located at the joint of two semicircular rings, and two ends of the gasket (5) are fixedly connected to the two semicircular rings via fastening nuts B (6).

3. The heat conduction device for laser additive manufacturing of dual alloy turbine disks according to claim 1, characterized in that: The rotating body (1) is made of copper and is a through-type structure.

4. The heat conduction device for laser additive manufacturing of a dual alloy turbine disk according to claim 1, characterized in that: The positioning protrusion (8) only extends to a depth of one third of the cooling air flow channel (7).

5. A laser additive manufacturing method for a dual alloy turbine disk, characterized in that: The heat conduction device according to any one of claims 1 to 4 is used, and the specific steps include: Step 1: performing initial polishing on the turbine disk body formed by laser selective melting and the blade area to be manufactured by additive manufacturing; using mechanical processing to remove the surface oxide film and ensure that the concentricity between the surface to be processed and the clamping end is not greater than 0.1 mm; Step 2: Perform fluorescence detection on the processing area, and there is no fluorescence display in the processing area; use an ultrasonic cleaning machine to clean and dry the parts, and mark the center line of the thickness direction of the processing surface; Step 3: Use 3D modeling software to process the blade model, and import it into 3dAMPPPlanner software to generate a printing trajectory and output the printing trajectory file layer by layer; Step 4: Install the heat conduction device of the disk body. First, insert a pair of rotating bodies (1) into the corresponding parts of the disk body and fix them with the fastening nut A (3) to ensure that they fit tightly with the disk body to prevent slippage when the disk body rotates; then assemble the two semicircular rings that make up the stationary body (2) onto the corresponding rotating body (1), and then splice them with the fastening nut B (6) and the gasket (5); finally, install the air inlet and air outlet pipes on the pair of connecting ports (4) located on the same stationary body (2) respectively; after the cooling tooling is installed, fix the parts on the processing table and adjust the coaxiality of the part processing surface to less than 0.2mm; Step 5: Take an appropriate amount of K477 powder with a particle size of 15 to 53 μm, dry the powder in an oven, and then pour it into the powder feeding device; Step 6: Use a fully enclosed inert gas protected laser direct deposition forming equipment to print the blade; after each layer of the blade is printed, wait for the substrate to cool down to below 50°C before printing the next layer; Step 7: Perform hot isostatic pressing + solid solution double aging treatment on the turbine disc after printing; Step 8: Process the dual alloy turbine disc blank into the required size according to the drawing.

6. The laser additive manufacturing method for a dual alloy turbine disk according to claim 5, characterized in that: In the step 5, the particle size of K477 powder is 15-53 μm, the oven baking temperature is 100° C., and the baking time is 1 hour.

7. The laser additive manufacturing method for a dual alloy turbine disk according to claim 5, characterized in that: The process parameters of step six are as follows: laser power 400-600W, powder feeding amount 2.5-3g / min, overlap rate 50%, filling scanning speed 650-750mm / min, contour scanning speed 400-500mm / min, powder feeding gas flow rate 8-10L / min, shielding gas flow rate 20-25L / min, the angle between the high-pressure turbine disk scanning trajectory and the positive direction of the X-axis is +20°-+30°, the angle between the low-pressure turbine disk scanning trajectory and the positive direction of the X-axis is -60--70°, the number of offset contours is 1-3, the scanning trajectory is a parallel line + contour offset, and the starting point is exchanged layer by layer.

8. The laser additive manufacturing method for a dual alloy turbine disk according to claim 5, characterized in that: In the step seven, the hot isostatic pressing system is: temperature 1150-1180°C, pressure 140-180MPa, and holding time 2-5h; the solid solution double aging system is: solid solution at 980°C, holding for 1h, then rapidly cooled to room temperature with argon, double aging at 720°C, holding for 8h, cooling to 620°C at 50°C / h, and then rapidly cooled to below 200°C with argon after holding for 8h.