Submerged-arc welding method for P690QL2 steel plate

Through the submerged arc welding method of P690QL2 steel plate, combined with specific welding parameters and process flow, the fatigue problem of P690QL2 steel plate under low temperature and high pressure conditions was solved, high strength, low temperature toughness and good mechanical properties were achieved, and -35℃ conditions were met The CTOD acceptance value requirements under the CTOD fill the technical gap in the field of low-temperature high-strength steel storage tank construction.

CN119016843APending Publication Date: 2024-11-26DALIAN SHIPBUILDING INDUSTRY CO LTD

Patent Information

Application Number
CN202411156513.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

P690QL2 steel plates are prone to fatigue problems under low temperature and high pressure conditions, and the existing welding technology is difficult to meet the requirements of high strength, low temperature toughness and fatigue performance, especially the CTOD test acceptance value under -35℃ conditions is insufficient.

Method used

The submerged arc welding method of P690QL2 steel plate is adopted, and the K-shaped bevel has an angle of 40° or 50° and a diameter of welding wire, and is made of argon arc vertical welding base welding, manual arc welding filling and submerged arc flat welding, combined with hydrogen removal The welding parameters are welding current 300~350A, voltage 28~32V, speed 300~400mm/min, heat input 13.0~22.4KJ/cm, preheating and welding wire drying, and the temperature between layers is controlled at 150℃~200℃.

Benefits of technology

It realizes the high strength, low temperature toughness and good mechanical properties of the welded joint under low temperature conditions, meets the requirement that the CTOD experimental value at -35℃ is not less than 0.2mm, avoids welding deformation and cracks, and improves welding efficiency and joints. resistant to fracture toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016843A_ABST
    Figure CN119016843A_ABST
Patent Text Reader

Abstract

A submerged-arc welding method for a P690QL2 steel plate comprises the steps that the P690QL2 steel plate with the thickness being 50 mm is adopted, a K-shaped groove is adopted, and welding wires and welding flux are matched for welding; the welding process comprises the steps that the front face of the groove is welded to a first preset position; turning over, performing carbon gouging polishing on the back surface of the groove, and then welding the back surface of the groove to a second preset position; turning over to complete the welding of the front surface of the groove, and then turning over to complete the welding of the back surface of the groove; hydrogen removal treatment is conducted in the welding process, and heat treatment is conducted after welding is completed; wherein submerged-arc welding is adopted in the welding process. When the welding process is used for welding the P690QL2 steel plate for the low-temperature and high-pressure container with the thickness of 50 mm, an obtained welding joint is excellent in strength and low-temperature toughness under the low-temperature condition, and the common mechanical performance requirements of stretching, impact, hardness, bending and the like can be met; and the requirements that the fracture toughness characteristic value and the CTOD experimental value at-35 DEG C are not less than 0.2 mm can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0003] The invention belongs to the field of ship construction and design, and particularly relates to a submerged arc welding method for a P690QL2 steel plate. Background Art

[0004] The low-carbon economy is an economic development model that, under the guidance of the concept of sustainable development, uses various means such as technological innovation, institutional innovation, industrial transformation, and new energy development to minimize the consumption of high-carbon energy such as coal and oil, reduce greenhouse gas emissions, and achieve a win-win situation for economic and social development and ecological environmental protection.

[0005] In recent years, carbon compliance, carbon recycling, and carbon trading have been put on the agenda, and the CO2-related industrial chain will become the next market hotspot. Due to the "three-phase" physical properties of CO2, it needs to be at a specific pressure and temperature to remain in a liquid state. Therefore, the material selection and application of its storage equipment are key. Low-temperature and high-strength pressure vessel steel P690QL2 is a better choice. Due to its excellent performance, P690QL2 material will be more commonly used in the field of CO2 low-temperature storage tanks. Therefore, research on P690QL2 steel welding technology is very necessary.

[0006] The yield limit of P690QL2 material reaches 690MPa, and the 50mm plate thickness exceeds the applicable range of IGC for tank materials (plate thickness less than 40mm, yield limit less than 410MPa). Marine cryogenic CO2 storage tanks are subjected to inertial loads caused by ship movement and produce fatigue problems. Generally, C-type tanks do not need to consider fatigue problems if they meet certain design pressure requirements, but for P690QL2, a high-strength rear plate that far exceeds the IGC requirements, its low-temperature toughness is very critical to ensure the fatigue performance of C-type tanks, and the classification society has very strict requirements on this. For DNV specifications, in addition to conventional welding test items, P690QL2 materials and their welds have added low-temperature impact tests and CTOD test items after post-weld heat treatment. The test temperature is -35°C and the CTOD test acceptance value must meet the requirement of ≥0.2. Summary of the invention

[0007] In order to solve the above problems, the present invention provides a submerged arc welding method for P690QL2 steel plate, aiming to achieve the purpose that high-strength thick plate welded joints can meet the requirements of fatigue performance, strength and low-temperature toughness in a low-temperature environment. The technical solution adopted is:

[0008] A submerged arc welding method for a P690QL2 steel plate. The P690QL2 steel plate adopts a K-type groove with a groove angle of 40° or 50°, a blunt edge of 2 mm, and a root gap of 0 to 5 mm.

[0009] The diameter is The welding wire is used to perform argon arc vertical welding on the front and back sides of the groove at the same time. The welding parameters of the base welding are: welding current 300-350A, welding voltage 28-31V, welding speed 300-350mm / min, and heat input 14.4-21.7KJ / cm.

[0010] After base welding, use a diameter of The welding wire is turned over and the front side of the groove is filled with manual arc welding vertically, and then the back side of the groove is turned over and the back side is filled with manual arc welding vertically. The parameters for manual arc welding on the front and back sides of the groove are: welding current 300~350A, welding voltage 29~32V, welding speed 300~400mm / min, heat input 13.0~22.4KJ / cm for welding.

[0011] After filling welding, the diameter of The welding wire is turned over and the front side of the groove is submerged arc welded to the predetermined position, and then the back side of the groove is turned over and submerged arc welded to the predetermined position. The parameters for submerged arc welding on the front and back sides of the groove are: welding current 300~350A, welding voltage 29~32V, welding speed 300~400mm / min, heat input 13.0~22.4KJ / cm for welding.

[0012] Dehydrogenation treatment is carried out during the welding process. The dehydrogenation treatment temperature is 250℃±25℃ and the treatment time is 2h. Heat treatment is carried out after welding is completed. The post-weld heat treatment temperature is 550℃±20℃ and the treatment time is 4h.

[0013] The above-mentioned submerged arc welding method of P690QL2 steel plate further comprises preheating the steel plate before welding, and the preheating temperature is not less than 150°C.

[0014] In the above-mentioned submerged arc welding method of P690QL2 steel plate, further, the welding wire is dried at 300° C. to 350° C. for 1 hour.

[0015] The above-mentioned submerged arc welding method of P690QL2 steel plate further has the following advantages: during the welding process, the interlayer temperature is not lower than 150°C and not higher than 200°C.

[0016] The above-mentioned submerged arc welding method of P690QL2 steel plate, further, the thickness of the P690QL2 steel plate is 50mm.

[0017] The above-mentioned submerged arc welding method of P690QL2 steel plate further has the impact energy of the steel plate base material at -60°C not less than 46J.

[0018] In the above-mentioned submerged arc welding method of P690QL2 steel plate, further, the welding material can be a welding rod or welding wire or welding flux of grade 5Y69H5.

[0019] The above-mentioned submerged arc welding method of the P690QL2 steel plate further requires that the P690QL2 steel plate be carbon planed and polished after each welding pass.

[0020] The technical advantage of the present invention is that the submerged arc welding process of the P690QL2 high-strength steel plate of the present invention adopts reasonable process parameters and post-weld heat treatment to reduce the degree of deformation caused by welding, ensure the overflow of diffused hydrogen, and avoid the generation of cracks. The outstanding advantage of this welding process method is that the submerged arc automatic welding has high welding efficiency, and is particularly suitable for flat welding and horizontal welding of thick plates and large-size equipment plates. At the same time, the mechanical properties of the welded joints of the P69QL2 steel plate used by the submerged arc welding method are better than those of the general manual arc welding method. According to the welding process of the present invention, it can be ensured that the weld has no welding defects, the tensile strength of the welded joint is not lower than that of the parent material, the bending performance is excellent, the Vickers hardness value of the parent material, the heat-affected zone, and the center of the weld is not higher than 420, and the Charpy impact value under -60°C is higher than 46J; in particular, a welded joint with good fracture toughness resistance can be obtained, which can meet the requirement that the CTOD test value is not less than 0.2mm under -35°C. The welding process of the present invention is used to weld 50mm thick P690QL2 low-temperature high-pressure container steel plates. The obtained welded joints have excellent strength and toughness under low temperature conditions, which can meet the general mechanical performance requirements such as tensile strength, impact, hardness, etc.; and can meet the requirement that the CTOD test value is not less than 0.2mm under -35°C conditions. Using the welding process of the present invention, after actual test verification after welding 50mm thick P690QL2 steel plates, the CTOD test under -35°C conditions meets the specification requirements, filling the gap in the field of P690QL2 low-temperature high-strength steel tank construction and promoting the development of low-temperature tank construction technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 Schematic diagram of the K-type groove used in the welding process of the present invention;

[0022] Figure 2 It is a schematic diagram of the welding process steps of the present invention;

[0023] Figure 3 This is a macroscopic overview of the welded joint obtained by the welding process of the present invention;

[0024] Figure 4 It is a schematic diagram of hardness test after welding by the welding process of the present invention;

[0025] Figure 5 It is a schematic diagram of the central fracture morphology of the weld after the welding process of the present invention is subjected to the CTOD test;

[0026] Figure 6 It is a schematic diagram of the fracture morphology of the heat-affected zone after welding by the welding process of the present invention in a CTOD test;

[0027] Among them: 1-base material, 2-heat affected zone, 3-weld. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with the accompanying drawings.

[0029] A welding method for P690QL2 steel plate is particularly suitable for welding medium-thickness P690QL2 steel plates for low-temperature and high-pressure containers. The base material of the welding process is a 50mm thick P690QL2 steel plate. The chemical composition and mechanical properties of the P690QL2 steel plate are shown in the following table.

[0030] Chemical composition:

[0031]

[0032] Mechanical properties:

[0033]

[0034] like Figure 1 As shown, K-type groove is used, the front groove angle is 40°, the back groove angle is 50°, the blunt edge is 2mm, and the root gap is 5mm. The welding material is selected to use the welding wire with the classification society certification level of 5Y69H5. The welding wire is dried at 300℃~350℃ for 1h. Before welding, the P690QL2 steel plate is preheated at a preheating temperature of 160℃. Figure 2As shown, after performing a layer of argon arc vertical welding base welding on the front side of the P690QL2 steel plate, the P690QL2 steel plate is turned over for carbon planing and grinding on the back side. After the carbon planing and grinding are completed, a layer of argon arc vertical welding base welding is performed on the back side of the P690QL2 steel plate. After the base welding, the P690QL2 steel plate is turned over for carbon planing and grinding on the front side. After the carbon planing and grinding are completed, the front side of the P690QL2 steel plate is filled with manual electric arc vertical welding, and then the P690QL2 steel plate is turned over for carbon planing and grinding on the back side. After the carbon planing and grinding are completed, the back side of the P690QL2 steel plate is filled with manual electric arc vertical welding. After filling welding, the P690QL2 steel plate is turned over for carbon planing and grinding on the front side. After carbon planing and grinding are completed, the front side of the P690QL2 steel plate is welded to the predetermined position for cover welding, and then the P690QL2 steel plate is turned over for carbon planing and grinding on the back side. After carbon planing and grinding are completed, the back side of the P690QL2 steel plate is welded to the predetermined position for submerged arc flat welding to complete the cover welding. The interlayer temperature plays the same role as the preheating temperature, and also affects the final organizational state of the weld. The interlayer temperature is not lower than the preheating temperature and not higher than 200℃.

[0035] The welding parameters used are as follows:

[0036]

[0037]

[0038] Welding materials:

[0039]

[0040] During welding, dehydrogenation treatment is carried out at a temperature of 250℃±25℃ for 2h. After welding, 100% appearance inspection, UT and MT inspection are carried out. After passing the inspection, post-weld heat treatment is carried out at a temperature of 550℃±20℃ for 4h.

[0041] In the above welding process, the impact energy of the steel plate base material at -60°C is not less than 46J.

[0042] The diameter of the welding rod and welding wire will affect the change of welding process parameters. The larger the diameter of the welding rod and welding wire, the greater the welding current and voltage will be. Therefore, the size of the columnar crystal and coarse crystal area in the weld area and heat-affected zone will increase. Therefore, the diameter of the argon arc base welding wire, the manual arc welding filling wire, and the submerged arc flat welding cover wire should be selected as of welding wire.

[0043] In order to ensure that a better low-temperature toughness joint is obtained, the selection of welding process parameters is crucial. Smaller heat input can obtain finer grains, and fine grain phases can increase the resistance to crack propagation, that is, increase the toughness of the material. However, this does not mean that the heat input can be reduced infinitely. Too low heat input will also produce unfavorable organizational morphology. In the present invention, after comparing the test results of several heat input ranges, it is determined that the better heat input range for submerged arc welding is 13.0-22.4KJ / cm.

[0044] Performance Testing

[0045] (1) Transverse tensile test of weld

[0046]

[0047]

[0048] (2) Weld longitudinal tensile test

[0049]

[0050] (3) Transverse bending test of weld

[0051]

[0052] (4) Impact test

[0053]

[0054] (5) Macroscopic test

[0055] Visual inspection of the macroscopic specimens after corrosion revealed no defects such as lack of fusion and cracks. The macroscopic appearance of the welded joints of the test plates can be seen in Figure 3 .

[0056] (6) Hardness test

[0057]

[0058]

[0059] (7) CTOD fracture toughness characteristic value detection

[0060] According to the specification requirements, three specimens were selected from the weld center and heat affected zone to conduct CTOD fracture toughness characteristic value tests at a temperature of -35°C. The test results are shown in the following table. Figure 5 As shown, the fracture morphology of the heat affected zone can be seen in Figure 6 shown.

[0061]

[0062]

[0063] The welding process of the present invention is used to weld 50mm thick P690QL2 steel plates for low-temperature and high-pressure containers. The resulting welded joints have excellent strength and low-temperature toughness under low-temperature conditions, which can meet the general mechanical properties requirements such as tension, impact, hardness, and bending; and can also meet the requirements that the fracture toughness characteristic value and the CTOD test value under -35°C conditions are not less than 0.2mm.

Claims

1. A submerged arc welding method for P690QL2 steel plate, characterized in that: The P690QL2 steel plate adopts a K-type groove with a front groove angle of 40° and a back groove angle of 50°, a blunt edge of 2mm, and a root gap of 0-5mm; Using a welding wire with a diameter of Æ 3.2mm, argon arc vertical welding is performed on the front and back sides of the groove at the same time. The welding parameters of the root welding are: welding current 300-350A, welding voltage 28-31V, welding speed 300-350mm / min, heat input 14.4-21.7KJ / cm; After the base welding, a welding wire with a diameter of Æ 3.2mm is used to turn over the front side of the groove for vertical manual arc welding filling, and then turn over the back side of the groove for vertical manual arc welding filling. The parameters for the manual arc welding on the front and back sides of the groove are: welding current 300-350A, welding voltage 29-32V, welding speed 300-400mm / min, heat input 13.0-22.4KJ / cm2 for welding; After the filling welding, a welding wire with a diameter of Æ 3.2mm is used to turn over the front side of the groove and perform submerged arc flat welding to the predetermined position, and then turn over the back side of the groove and perform submerged arc flat welding to the predetermined position. The parameters for submerged arc flat welding on the front and back sides of the groove are: welding current 300-350A, welding voltage 29-32V, welding speed 300-400mm / min, heat input 13.0-22.4KJ / cm for welding; Dehydrogenation treatment is carried out during the welding process. The dehydrogenation treatment temperature is 250℃±25℃ and the treatment time is 2h. Heat treatment is carried out after welding is completed. The post-weld heat treatment temperature is 550℃±20℃ and the treatment time is 4h.

2. The submerged arc welding method of a P690QL2 steel plate according to claim 1, characterized in that: Before welding, the steel plate should be preheated at a temperature not lower than 150°C.

3. The submerged arc welding method of a P690QL2 steel plate according to claim 1, characterized in that: The welding wire is dried at 300℃~350℃ for 1h.

4. The submerged arc welding method of a P690QL2 steel plate according to claim 1, characterized in that: During welding, the interlayer temperature shall not be lower than 150°C and not higher than 200°C.

5. The submerged arc welding method of P690QL2 steel plate according to claim 1, characterized in that: The thickness of P690QL2 steel plate is 50mm.

6. The submerged arc welding method of P690QL2 steel plate according to claim 1, characterized in that: The impact energy of the steel plate base material at -60℃ shall not be less than 46J.

7. The submerged arc welding method of P690QL2 steel plate according to claim 1, characterized in that: The welding material may be a welding rod or welding wire or welding flux of grade 5Y69H5.

8. The submerged arc welding method of P690QL2 steel plate according to claim 1, characterized in that: After each welding process is completed, the P690QL2 steel plate needs to be carbon planed and polished.

Citation Information

Patent Citations

  • Girth welding technology for vacuum container

    CN102357741A

  • Equal-intensity matching welding rod manual welding method for P690QL1 high-intensity steel

    CN103464865A

  • Method of common automatic submerged-arc welding machine for welding small-diameter barrel butting seams

    CN104308340A

  • Welding method for P690QL1 steel flux-cored wire gas metal arc welding

    CN110270745A

  • 304L austenitic stainless steel MIG welding method

    CN111230264A

Cited By

  • Efficient welding method

    CN119387772A

  • An efficient welding method

    CN119387772B

  • Welding process for large and thick ultrahigh-strength steel plate of offshore wind power pipe pile

    CN122164982A