Preparation method and die for variable-cross-section asymmetric arc-shaped complex stainless steel forge piece

By employing a multi-step slab welding and bending forming method, combined with heat treatment and mold use, the problems of low material utilization and low efficiency in complex arc-shaped stainless steel forgings with variable cross-section and asymmetry were solved, achieving efficient and precise forming.

CN119017008AActive Publication Date: 2024-11-26TIANJIN HEAVY EQUIP ENG RES +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310607185.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

Existing technologies suffer from low material utilization, high cost, and low efficiency when preparing complex arc-shaped stainless steel forgings with variable cross-sections and asymmetry, especially for irregularly shaped complex austenitic stainless steel forgings which are difficult to form precisely.

Method used

The method involves welding slabs with multi-step structures into symmetrical components and then bending them. This is combined with stepped homogenization heat treatment, limiting upsetting and drawing parameters, and heat preservation before bending. A mold is used for bending, and finally the components are disassembled into the required structures.

Benefits of technology

It improves material utilization, reduces subsequent processing allowance, increases production efficiency, solves the problem of bending instability of individual asymmetrical slabs, and enhances the thermoplasticity and precision of forgings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017008A_ABST
    Figure CN119017008A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method and a die for a variable-cross-section asymmetric arc-shaped complex stainless steel forge piece, belongs to the technical field of stainless steel forge piece manufacturing, and solves the problems of low material utilization rate and low efficiency of an existing method. The preparation method comprises the following steps: step 1, cogging and forging a steel ingot; 2, plate blank forging is conducted, a pair of plate blanks is forged, one face of each plate blank is of a multi-step structure, and the other face of each plate blank is a plane; 3, the faces, with the multi-step structures, of the two plate blanks are oppositely placed, the steps corresponding to the maximum cross sections of the two plate blanks are installed and welded, and the installed and welded assembly is a symmetrical assembly; 4, the symmetrical assembly is subjected to bending forming; and 5, the steps corresponding to the maximum cross sections of the two plate blanks are split, then the multi-step structure of each plate blank is machined into the structure needed by the part, and the two variable-cross-section asymmetric arc-shaped complex stainless steel forgings are obtained. The method is high in material utilization rate and high in preparation efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of stainless steel forging manufacturing, and in particular to a preparation method and a die for a variable-section asymmetric arc-shaped complex stainless steel forging. Background Art

[0002] Stainless steel forgings are widely used in mechanical equipment and other fields. For low-temperature resistant non-magnetic austenitic materials with variable cross-section, asymmetric arc-shaped complex stainless steel forgings, on the one hand, due to their complex shape, forging is very difficult. On the other hand, the austenitic stainless steel material itself has the characteristics of high deformation resistance and poor thermoplasticity, which makes it difficult to achieve the goal of precise forming of special-shaped complex austenitic stainless steel forgings.

[0003] The existing method for forging asymmetric arc-shaped stainless steel forgings with variable cross-sections is to adopt a large excess covering forging method, first prepare a rectangular ingot, then bend the ingot to form an arc, and then forge the ingot into a variable cross-section asymmetric structure of the target part. The forged forging blank is a simple shape structure, and finally the excess blank is removed by machining. However, this method has a large ingot excess, low material utilization, high cost, and only one forging is produced at a time, which is inefficient. Summary of the invention

[0004] In view of the above analysis, an embodiment of the present invention aims to provide a method and mold for preparing a variable-section asymmetric arc-shaped complex stainless steel forging, so as to solve at least one of the following problems of the existing method: (1) large machining allowance, low material utilization rate and high cost; (2) only one forging is produced at a time, which is inefficient.

[0005] On the one hand, an embodiment of the present invention provides a method for preparing a variable-section asymmetric arc-shaped complex stainless steel forging, the preparation method comprising:

[0006] Step 1: Forging the steel ingot;

[0007] Step 2: forging a pair of slabs, wherein one side of each slab has a multi-step structure and the other side is a plane;

[0008] Step 3: Place the surfaces of the two slabs with multi-step structures opposite to each other, and weld the steps corresponding to the maximum cross-sections of the two slabs. The welded assembly is a symmetrical assembly.

[0009] Step 4: bending the symmetrical component;

[0010] Step 5: Split the steps corresponding to the maximum cross-section of the two slabs, and then process the multi-step structure of each slab into the structure required by the part to obtain two variable-section asymmetric arc-shaped complex stainless steel forgings.

[0011] Preferably, in step 1, before the steel ingot is forged, the steel ingot is first subjected to homogenization heat treatment.

[0012] Preferably, the homogenization heat treatment adopts a step-by-step heating method, including: a first temperature step of 840-860°C, a second temperature step of 1050-1060°C, and a third temperature step of 1200-1220°C.

[0013] Preferably, in step 1, the blank forging includes at least one upsetting deformation and at least one drawing deformation;

[0014] The forging ratio of the upsetting deformation is not less than 1.7, and the forging ratio of the drawing deformation is not less than 1.7.

[0015] Preferably, in step 2, the multi-step structure is a gradually descending or gradually increasing multi-step structure extending from one end to the other end of the slab.

[0016] Preferably, in step 2, the forging ratio of each step in the multi-step structure is not less than 1.3.

[0017] Preferably, in step 4, before the symmetrical forging is bent and formed, the symmetrical component is firstly kept warm below the secondary recrystallization temperature.

[0018] Preferably, step 3 further comprises: welding lifting ears at both ends of two plate blanks constituting the symmetrical component.

[0019] On the other hand, the present invention further provides a mold, which is used in the bending forming step in the above-mentioned preparation method, and the mold includes an upper mold and a lower mold;

[0020] A surface of the upper die opposite to the lower die is a curved surface;

[0021] The lower mold comprises a square base and columns arranged at four corners of the base, and each column is provided with a groove.

[0022] Preferably, the curvature of the arc surface of the upper die is the same as the arc curvature of the variable-section asymmetric arc-shaped complex stainless steel forging.

[0023] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0024] 1. The method of the present invention first forges a steel ingot into a slab with a multi-step structure on one side, then welds two slabs into a symmetrical assembly, then bends the symmetrical assembly, and finally splits it to process the multi-step structure of each slab into the structure required by the part. The slab with a multi-step structure is closer to the final part shape, which can effectively improve the material utilization rate and reduce the subsequent processing allowance. The processing allowance of each part is less than 40 mm. In a preferred embodiment, the processing allowance of each part is less than 20 mm.

[0025] 2. In the method of the present invention, two forgings can be prepared in one bending forming process, thereby improving production efficiency. Especially for the need to prepare a pair of complex stainless steel forgings with asymmetric arc shapes and variable cross-sections, the method of the present invention can prepare a pair of forgings in one bending forming process, thereby improving parts production efficiency.

[0026] 3. The present invention welds two single asymmetric slabs into a symmetrical assembly and then bends them to form them, which can effectively solve the problem of bending instability of a single asymmetric slab.

[0027] 4. The present invention improves the grain refinement of the forging (the grain size in the microstructure is 1-3 levels, and in a preferred embodiment, the grain size in the microstructure is 4-5 levels) by performing step-by-step homogenization heat treatment on the forging, limiting the upsetting and drawing parameters, and heating and heat preservation below the secondary recrystallization temperature before bending forming, so that the forging has better thermoplasticity, thereby improving the forging accuracy.

[0028] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0030] Figure 1 This is the steel ingot homogenization heat treatment process in step 1 of the present invention;

[0031] Figure 2 The process of the open blank forging in step 1 and the multi-step slab forging in step 2 of the present invention;

[0032] Figure 3 The slab forging with a multi-step structure obtained in step 2 of the present invention;

[0033] Figure 4The symmetrical assembly is obtained by welding two slabs in step 3 of the present invention;

[0034] Figure 5 This is the process of bending the symmetrical component in step 4 of the present invention;

[0035] Figure 6 This is a schematic diagram of splitting two slabs in step 5 of the present invention;

[0036] Figure 7 This is a schematic diagram of the structure required for forging the multi-step structure of the slab into a part in step 5 of the present invention;

[0037] Figure 8 This is the final parts schematic diagram;

[0038] Fig. 9 It is a schematic diagram of the mold structure of the present invention.

[0039] Fig.10 It is a flow chart of a method for preparing a variable cross-section asymmetric arc-shaped complex stainless steel forging in the prior art;

[0040] Fig.11 Schematic diagram of slab assembly welding in step 3 of the present invention;

[0041] Fig.12 The metallographic photograph of the forging was obtained in Example 2 of the present invention.

[0042] Reference numerals:

[0043] 1-upper die; 2-lower die; 201-square base; 202-column; 203-groove. DETAILED DESCRIPTION

[0044] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0045] On the one hand, the present invention provides a method for preparing a variable cross-section asymmetric arc-shaped complex stainless steel forging, such as Figure 1-Figure 7 As shown, the preparation method comprises:

[0046] Step 1: Forging the steel ingot;

[0047] Step 2: forging a pair of slabs, wherein one side of each slab has a multi-step structure and the other side is a plane;

[0048] Step 3: Place the surfaces of the two slabs with multi-step structures opposite to each other, and weld the steps corresponding to the maximum cross-sections of the two slabs. The welded assembly is a symmetrical assembly.

[0049] Step 4: bending the symmetrical component;

[0050] Step 5: Split the steps corresponding to the maximum cross-section of the two slabs, and then process the multi-step structure of each slab into the structure required by the part to obtain two variable-section asymmetric arc-shaped complex stainless steel forgings.

[0051] Compared with the prior art, the method of the present invention first forges the steel ingot into a slab with a multi-step structure on one side, and then welds the two slabs into a symmetrical assembly, and then bends the symmetrical assembly, and finally splits it to forge the multi-step structure of each slab into the structure required by the part. The slab with a multi-step structure is closer to the final part shape, which can effectively improve material utilization and reduce subsequent processing allowances. In the method of the present invention, two forgings can be prepared in one bending forming process, which improves production efficiency. In particular, for a pair of complex stainless steel forgings with asymmetric arc shapes with variable cross-sections, the method of the present invention can prepare a pair of forgings in one bending forming process, which improves part production efficiency. The pair of forgings refers to two symmetrical forgings, for example, Figure 8 The two opposite side forgings of the box body shown in the figure can be prepared by the method of the present invention at one time. The present invention welds two single asymmetric slabs into a symmetrical assembly and then bends them, which can effectively solve the problem of bending instability of a single asymmetric slab.

[0052] Exemplarily, the stainless steel forging is a low-temperature resistant non-magnetic austenitic stainless steel forging.

[0053] Since austenitic stainless steel material itself has the characteristics of high deformation resistance and poor thermoplasticity, it is difficult to achieve precise forming of special-shaped and complex austenitic stainless steel forgings.

[0054] In the present invention, in order to promote the precise forming of the variable cross-section asymmetric arc-shaped complex stainless steel forgings, in the step 1, before the steel ingot is forged, the steel ingot is first subjected to homogenization heat treatment.

[0055] Specifically, Figure 1 As shown, the homogenization heat treatment adopts a step-by-step heating method, including: a first temperature step of 840-860°C, a second temperature step of 1050-1060°C, and a third temperature step of 1200-1220°C.

[0056] It should be noted that insulation is carried out at each temperature step, and the insulation time is determined according to the smallest position cross-section. The minimum insulation time is determined at one hour per 80 mm, and the maximum insulation time is determined at one hour per 50 mm.

[0057] Specifically, the first temperature step is the mutation point of the thermal expansion coefficient. After being kept and heated at this temperature, it is raised to the second temperature step. The heat preservation and heating at the second temperature step will not cause obvious grain growth. Then, the high temperature heat preservation at the third temperature step is to provide the necessary conditions for the deformation of the blank forging. In addition, the homogenization heat treatment adopts a step-by-step heating method, and the first and second temperature steps are kept for a period of time, which can make the segregation elements pre-diffused and avoid the initial melting of the grain boundaries. Then, it is raised to the third step and kept for a certain period of time, which can gradually eliminate segregation and dendrites, improve the thermoplasticity of austenitic stainless steel, reduce forging cracking, and achieve small margin precision forging.

[0058] Furthermore, before the homogenization heat treatment, the slag grooves on the surface of the steel ingot are removed, which can effectively avoid the subsequent forging cracking problem caused by the slag grooves.

[0059] For example, Figure 2 As shown, in step 1, the blank forging includes at least one upsetting deformation and at least one drawing deformation. Blank forging mainly breaks up the cast structure of the ingot, generates a large number of dislocations and slips, is more conducive to the diffusion of elements, can further eliminate segregation, and further improve the thermoplasticity of austenitic stainless steel.

[0060] Exemplarily, the forging ratio of the upsetting deformation is not less than 1.7 (e.g., 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, etc.), and the final forging temperature is higher than 900°C (e.g., 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C, etc.). A forging ratio of 1.7 or more can ensure sufficient large deformation and meet the requirements of fine and uniform grains; the final forging temperature is higher than 900°C to avoid cracking. If it is lower than 900°C, the degree of cracking tendency will increase.

[0061] It should be noted that before the forging billet after upsetting deformation is returned to the furnace, it is wrapped with asbestos anvils for heat preservation and forging, so as to avoid too fast temperature drop during the forging process and extend the effective forging time. After the insulation is completed, the upper and lower wide flat anvils are used for drawing and deformation.

[0062] Exemplarily, the forging ratio of the elongation deformation is not less than 1.7 (e.g., 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, etc.), the final forging temperature is higher than 900°C (e.g., 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C, etc.), and the asbestos anvil is wrapped around the forging blank before returning to the furnace for heat preservation forging to avoid too fast temperature drop during the forging process, which can extend the effective forging time. A forging ratio of more than 1.7 can ensure sufficient large deformation and meet the requirements of fine and uniform grains; the final forging temperature is higher than 900°C to avoid cracking. If it is lower than 900°C, the degree of cracking tendency will increase.

[0063] It should be noted that Figure 2 and Figure 3 Only one multi-step structure is shown, but the multi-step structure of the present invention is not limited thereto.

[0064] Exemplarily, in step 2, the specific shape of the multi-step structure can be determined according to the variable-section asymmetric structure of the target part. For example, the multi-step structure is a multi-step structure that gradually descends or gradually increases from one end of the slab to the other end, or a multi-step structure that first increases and then descends, or a multi-step structure that first descends and then increases. Figure 2 and Figure 3 The multi-step structure in Figure 8 Side panels and Figure 7 The variable cross-section asymmetric structure of the target part in the model is the slope structure in the part. The multi-step shape slab is closer to the final part shape, which can effectively improve material utilization and reduce subsequent processing allowance.

[0065] Exemplarily, in step 2, a pair of multi-step shaped slabs are drawn out using upper and lower flat anvils, and the forging ratio of each step in the multi-step structure is not less than 1.3, for example, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, etc., to meet the critical deformation amount of dynamic recrystallization of the material and achieve grain refinement.

[0066] For example, in step 3, the welding method includes: processing 10×10 mm welding grooves on four sides of the corresponding welding surface, and then butt welding the two plate blanks, such as Fig.11 shown.

[0067] Exemplarily, in order to facilitate lifting, step 3 further includes: welding lifting ears at both ends of two slabs constituting the symmetrical component.

[0068] For example, in step 4, before the symmetrical component is bent, the symmetrical component is first kept warm below the secondary recrystallization temperature, and the holding time is determined as 1 hour per 80 mm at the thickest section. Heating and keeping warm below the secondary recrystallization temperature can effectively avoid the problem of grain growth of austenitic stainless steel and further improve thermoplasticity.

[0069] Exemplarily, in step 5, the splitting method includes: splitting by gouging the original weld position.

[0070] Exemplarily, in step 5, the method of processing the multi-step structure of each slab into the structure required by the part may be machining.

[0071] In a second aspect, the present invention also provides a mold, such as Fig. 9As shown, the mold is used in the bending forming step in the above-mentioned preparation method, and the mold includes an upper mold 1 and a lower mold 2;

[0072] The surface of the upper mold 1 opposite to the lower mold 2 is a curved surface;

[0073] The lower mold 2 includes a square base 201 and columns 202 arranged at four corners of the base 201 , and each column 202 is provided with a groove 203 .

[0074] Specifically, the curvature of the arc surface of the upper die 1 is the same as the arc curvature of the variable-section asymmetric arc-shaped complex stainless steel forging.

[0075] Exemplarily, the length of the square base 201 is not less than the length of the symmetrical component, and the width of the square base 201 is not less than the width of the symmetrical component. The groove 203 is used to support the two ends of the two slabs in the symmetrical component; the height of each column 202 is such that the symmetrical component has enough space when bending downward.

[0076] When the mold is applied to step 4 of the preparation method of the present invention, Figure 5 As shown, the symmetrical component is placed on the lower mold 2, and the two ends of the two slabs in the symmetrical component are placed in the corresponding grooves 203 respectively. The upper mold 1 is used to press down from the upper surface of the symmetrical component until the bending deformation of the symmetrical component is completed.

[0077] The following is a further explanation of the method for preparing the variable cross-section asymmetric arc-shaped complex stainless steel forging of the present invention through specific embodiments.

[0078] Example 1

[0079] This embodiment provides a mold, the mold comprising an upper mold 1 and a lower mold 2;

[0080] The surface of the upper mold 1 opposite to the lower mold 2 is a curved surface;

[0081] The lower mold 2 includes a square base 201 and columns 202 arranged at four corners of the base 201 , and each column 202 is provided with a groove 203 .

[0082] The curvature of the arc surface of the upper die 1 is the same as the arc curvature of the variable-section asymmetric arc-shaped complex stainless steel forging.

[0083] The length of the square base 201 is not less than the length of the symmetrical component, and the width of the square base 201 is not less than the width of the symmetrical component. The groove 203 is used to support the two ends of the two slabs in the symmetrical component; the height of each column 202 allows the symmetrical component to have enough space when bending downward.

[0084] Example 2

[0085] This embodiment provides a method for preparing a variable cross-section asymmetric arc-shaped complex stainless steel forging, wherein the variable cross-section asymmetric arc-shaped complex stainless steel forging is as follows Figure 8 The two side plate forgings of the box body shown are made of 316LN, and each side plate forging is a complex arc-shaped structure with a variable cross-section, such as Figure 2 The forging weighs about 4 tons and is made from 6 tons of electroslag steel ingots.

[0086] 1. Pre-treat the electroslag ingot, and remove the surface slag grooves after annealing.

[0087] 2. The electroslag ingot is subjected to homogenization heat treatment, which adopts a step-by-step heating method, with the first temperature step being 850°C, the second temperature step being 1055°C, and the third temperature step being 1210°C. Insulation is performed at each temperature step, and the insulation time is determined as one hour per 60mm.

[0088] 3. Steel ingot forging, such as Figure 2 As shown, the steel ingot is first upset with an upsetting ratio of 1.7 and a final forging temperature of 1000°C. The forging blank is wrapped with an asbestos anvil before returning to the furnace. After the insulation is completed, the upper and lower wide flat anvils are used for drawing. The drawing ratio is 1.7 and the final forging temperature is higher than 1000°C. The forging blank is wrapped with an asbestos anvil before returning to the furnace.

[0089] 4. A pair of slabs are drawn out using upper and lower flat anvils, one side of each slab having a multi-step structure and the other side being a flat surface; the multi-step structure is a gradually descending multi-step structure extending from one end of the slab to the other end, such as Figure 2 and Figure 3 As shown; the forging ratio of each step in the multi-step structure is 1.5.

[0090] 5. Place the surfaces of the two slabs with multi-step structures opposite to each other, and weld the steps corresponding to the maximum cross-sections of the two slabs. The welded components are symmetrical components, such as Figure 4 As shown, lifting ears are welded at both ends of the two plate blanks constituting the symmetrical component.

[0091] 6. The symmetrical component is kept warm below the secondary recrystallization temperature. After the warming is completed, the mold of Example 1 is used to bend the symmetrical component, such as Figure 5 As shown, the symmetrical component is placed on the lower die, the two ends of the two plate blanks in the symmetrical component are placed in the corresponding grooves respectively, and the upper die is used to press down from the upper surface of the symmetrical component until the bending deformation of the symmetrical component is completed.

[0092] 7. Such as Figure 6 As shown, the steps corresponding to the maximum cross-sections of the two slabs are split, as shown in Figure 7As shown, the multi-step structure of each slab is then machined into a slope structure to obtain two variable-section asymmetric arc-shaped complex stainless steel forgings, namely, Figure 8 The two side plate forgings of the box body are shown.

[0093] The embodiment does not experience bending instability during the bending deformation process; the grain size in the microstructure of the forging is 4-5, and the grains are fine and uniform. Fig.12 As shown in the figure, forging accuracy refers to the machining allowance from the forging blank to the final structural parts, and the machining allowance of each part is less than 20mm.

[0094] Example 3

[0095] This embodiment provides a method for preparing a variable-section asymmetric arc-shaped complex stainless steel forging similar to Embodiment 2, except that the homogenization heat treatment is not a step-by-step heating method, but a direct heating to 1210°C.

[0096] The microstructure of the forging obtained in this embodiment has a grain size of 1-3, with a small amount of mixed crystals and coarse crystals, and the machining allowance of each part is 30-40 mm.

[0097] Example 4

[0098] This embodiment provides a method for preparing a variable cross-section asymmetric arc-shaped complex stainless steel forging similar to Embodiment 2, except that the final forging temperature of upsetting and squaring is 800°C.

[0099] The forging obtained in this embodiment has a small amount of cracks on its surface.

[0100] Example 5

[0101] This embodiment provides a method for preparing a variable-section asymmetric arc-shaped complex stainless steel forging similar to that of Embodiment 2, except that the surface slag grooves of the electroslag ingot are not removed before the homogenization heat treatment.

[0102] The forging obtained in this embodiment has a small amount of cracks on its surface.

[0103] Example 6

[0104] This embodiment provides a method for preparing a variable-section asymmetric arc-shaped complex stainless steel forging similar to Embodiment 2, except that before the symmetrical component is bent and formed, the symmetrical component is kept warm at a temperature exceeding the secondary recrystallization temperature.

[0105] The grain size in the microstructure of the forging obtained in this embodiment is level 1-3.

[0106] Comparative Example 1

[0107] This comparative example provides a method for preparing an existing variable cross-section asymmetric arc-shaped complex stainless steel forging. Figure 8 The two side plate forgings of the box body shown in the figure. Fig.10 As shown, the method includes: first preparing a rectangular steel ingot, then bending the steel ingot to form an arc, and then forging the bent steel ingot into a variable-section asymmetric structure of a target part, the forged forging blank finished product is a simple shape structure, and finally machining is used to remove excess blank.

[0108] The grain size in the microstructure of the forging prepared in this comparative example is level 1-2, and the machining allowance of each part is 20-300 mm.

[0109] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for preparing a complex stainless steel forging with asymmetric variable cross-section and arc shape. It is characterized in that The preparation method comprises: Step 1: Forging the steel ingot; Step 2: forging a pair of slabs, wherein one side of each slab has a multi-step structure and the other side is a plane; Step 3: Place the surfaces of the two slabs with multi-step structures opposite to each other, and weld the steps corresponding to the maximum cross-sections of the two slabs. The welded assembly is a symmetrical assembly. Step 4: bending the symmetrical component; Step 5: Split the steps corresponding to the maximum cross-section of the two slabs, and then process the multi-step structure of each slab into the structure required by the part to obtain two variable-section asymmetric arc-shaped complex stainless steel forgings.

2. The preparation method according to claim 1, It is characterized in that In the step 1, before the steel ingot is forged, the steel ingot is first subjected to a homogenization heat treatment.

3. The preparation method according to claim 2, It is characterized in that The homogenization heat treatment adopts a step-by-step heating method, including: a first temperature step of 840-860°C, a second temperature step of 1050-1060°C, and a third temperature step of 1200-1220°C.

4. The preparation method according to claim 1, It is characterized in that In the step 1, the blank forging includes at least one upsetting deformation and at least one drawing deformation; The forging ratio of the upsetting deformation is not less than 1.7, and the forging ratio of the drawing deformation is not less than 1.

7.

5. The preparation method according to claim 1, It is characterized in that In step 2, the multi-step structure is a gradually descending or gradually increasing multi-step structure extending from one end to the other end of the slab.

6. The preparation method according to claim 1, It is characterized in that In step 2, the forging ratio of each step in the multi-step structure is not less than 1.

3.

7. The preparation method according to claim 1, It is characterized in that In step 4, before the symmetrical component is bent and formed, the symmetrical component is firstly kept warm below the secondary recrystallization temperature.

8. The preparation method according to claim 1, It is characterized in that Step 3 also includes: welding lifting ears at both ends of the two plate blanks constituting the symmetrical component.

9. A mold, which is used in the bending forming step in the preparation method according to claims 1 to 8, It is characterized in that The mold comprises an upper mold (1) and a lower mold (2); The surface of the upper mold (1) opposite to the lower mold (2) is a curved surface; The lower mold (2) comprises a square base (201) and columns (202) arranged at four corners of the base (201), and each column (202) is provided with a groove (203).

10. The mold according to claim 9, It is characterized in that The curvature of the arc surface of the upper die (1) is the same as the arc curvature of the variable-section asymmetric arc-shaped complex stainless steel forging.

Citation Information

Patent Citations

  • Manufacturing method of double-curved-surface fish-bellied continuous box beam variable-cross-section steel moulding plate

    CN109352285A

  • Complex arc-shaped variable-cross-section forge piece forging and rolling forming method

    CN109365700A

  • Free forging machining method of aircraft aluminum alloy arc forged plate

    CN112676504A

  • COMPOSITE STEEL MATERIAL AND METHOD FOR ITS MANUFACTURING.

    NO892508D0