Preparation process of super-flexible sizing pipe for fuel gas

Through multi-layer coextrusion technology and precise control of nanocomposite materials and high-density polyethylene, the problems of gas pipes in mechanical properties, chemical corrosion resistance and production efficiency are solved, and high-quality and high-performance gas super-purpose Preparation of flexible ruler tube.

CN119017670APending Publication Date: 2024-11-26ZHENLAN PIPE TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411120762.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing gas pipes have shortcomings in mechanical properties, chemical corrosion resistance, production efficiency and quality control, especially in extreme environments, performance degradation, inaccurate temperature control, inconsistent multi-layer coextrusion technology, lack of online monitoring and Automatic adjustment system results in high scrap rate and low production reliability.

Method used

The mixture of nanocomposite materials and high-density polyethylene is achieved through multi-layer coextrusion technology and precise temperature control, combined with intelligent cooling system, servo motor stretching and laser cutting, plasma processing and high-resolution detection system. Uniformity and interlayer adhesion ensure product quality and production efficiency.

Benefits of technology

It significantly improves the mechanical strength, chemical corrosion resistance and production efficiency of the pipe, ensures high quality and consistency of the product, extends service life, reduces internal stress and physical deformation, and improves coating adhesion and protection performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017670A_ABST
    Figure CN119017670A_ABST
Patent Text Reader

Abstract

The invention relates to the field of plastic processing, and discloses a fuel gas super-soft sizing pipe preparation process which comprises the following steps: a) providing raw materials: mixing high-density polyethylene with a nano material; b) pretreatment of the composite material: pre-mixing the raw materials in a high-shear mixer, and carrying out fusion treatment in a double-screw extruder at a constant temperature; c) extrusion molding: arranging a precisely controlled three-layer co-extrusion head in an extruder, and extruding the composite material in a temperature range of 210-230 DEG C to form a multi-layer structure pipe; and d) a multi-layer co-extrusion structure: the outer layer is made of an anti-aging polymer containing a UV stabilizer, the middle layer is made of a nano composite reinforcing material, and the inner layer is made of a chemical corrosion resistant material. The high-density polyethylene is mixed with the nano clay and the nano silicon dioxide, so that the mechanical strength, the wear resistance and the chemical corrosion resistance of the pipe are remarkably enhanced. By using the nano composite material, the problem that the pipe is easy to damage in a harsh environment is effectively solved, the service life of the pipe is prolonged, and the safety of the pipe is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of plastic processing, in particular to a preparation process of an ultra-flexible fixed-length pipe for gas. Background Art

[0002] In the field of gas pipe production, especially in the preparation of ultra-flexible cut-to-length pipes, existing technologies face multiple challenges, mainly in terms of material properties, production efficiency and product quality control. Traditional preparation processes usually use a single material such as ordinary high-density polyethylene (HDPE), which, although showing good performance in certain applications, often cannot meet higher industrial standards in terms of durability, mechanical strength and chemical stability. In addition, existing production technologies have limitations in terms of temperature control, material uniformity and precision processing, which affect the overall quality and performance of the product.

[0003] The main shortcomings of the existing technology include:

[0004] Material performance limitations: The materials used in existing technologies are mostly ordinary polymers without reinforcement, such as HDPE. Although these materials have basic physical and chemical properties, they are prone to performance degradation in extreme environments (such as high temperature, high pressure or chemical corrosion environments). The lack of necessary reinforcement measures, such as the use of nanocomposites, limits the application range and life of pipes.

[0005] Imprecise processing control: In the traditional extrusion process, temperature control is often not precise enough, and temperature fluctuations in the extrusion equipment may lead to unstable material properties, affecting the mechanical and chemical properties of the pipe. In addition, the application of multi-layer co-extrusion technology is not common, resulting in the inability to effectively produce composite structure pipes with specific functional layers.

[0006] Production efficiency and quality control issues: The traditional process lacks effective online monitoring and automatic adjustment systems, resulting in low production efficiency and large fluctuations in product quality. Real-time quality control during the production process, such as online wall thickness detection and surface quality assessment, is not implemented, which leads to high scrap rates and low production reliability.

[0007] Poor environmental adaptability: Existing technologies fail to provide adequate environmental adaptability, especially in terms of resistance to ultraviolet radiation and chemical corrosion. Existing pipes are prone to material aging, color change and performance degradation after long-term exposure to the external environment.

[0008] Therefore, the present invention proposes a process for preparing an ultra-flexible fixed-length pipe for gas to solve the deficiencies of the prior art. Summary of the invention

[0009] In view of the shortcomings of the prior art, the present invention provides a process for preparing ultra-flexible fixed-length pipes for gas, which solves the problems of existing pipes in terms of mechanical properties, chemical corrosion resistance, production efficiency and quality control. The present invention significantly improves the comprehensive performance and production efficiency of gas pipes by introducing nanocomposites, applying multi-layer co-extrusion technology, precise temperature and flow rate control, and advanced online detection and surface treatment technology.

[0010] To achieve the above objectives, the present invention is implemented through the following technical solutions: A process for preparing an ultra-flexible fixed-length pipe for gas, comprising the following steps:

[0011] a) Providing raw materials: mixing high-density polyethylene with nanomaterials;

[0012] b) Pretreatment of composite materials: premixing the raw materials in a high shear mixer and fusing them at a constant temperature in a twin-screw extruder;

[0013] c) Extrusion molding: The extruder is equipped with a precisely controlled three-layer co-extrusion head to extrude the composite material at a temperature range of 210°C to 230°C to form a multi-layer structure pipe;

[0014] d) Multi-layer co-extrusion structure: the outer layer uses an aging-resistant polymer containing UV stabilizer, the middle layer is a nano-composite reinforcement material, and the inner layer is a chemical corrosion-resistant material;

[0015] e) Intelligent cooling system: through the segmented cooling pipe equipped with temperature and flow rate sensors, the state of the cooling medium is monitored and adjusted in real time to ensure the uniformity of material properties;

[0016] f) Synchronous stretching and cutting to length: The stretching ratio is adjusted to 1.2 using a servo motor-controlled stretching device, followed by cutting to length using laser cutting technology with an accuracy of ±0.1 mm;

[0017] g) Surface treatment and functionalization: plasma treatment with a power of 150 watts and a treatment time of 1-3 seconds to improve the adhesion of the coating;

[0018] h) Online intelligent detection: Using visual inspection system and ultrasonic thickness measurement equipment, set the sampling frequency to 200 times per second, real-time monitoring and automatic adjustment of production parameters based on the results.

[0019] Preferably, the nanomaterials include nanoclay and nanosilicon dioxide, and the total proportion of the nanomaterials is 2% to 4% of the total weight of the substrate.

[0020] Preferably, the rotation speed of the high shear mixer is 4000 to 6000 revolutions per minute; and the temperature of the twin-screw extruder is controlled at 215° C. to 225° C.

[0021] Preferably, the multi-layer co-extrusion structure has an outer layer thickness of 0.5 mm to 1 mm, a middle layer thickness of 2 mm to 3 mm, and an inner layer thickness of 0.5 mm to 1 mm.

[0022] Preferably, the aging-resistant polymer is selected from high-density polyethylene, polypropylene or a combination thereof; the nanocomposite reinforcing material is selected from nanoclay, nanosilica or a combination thereof; the chemical corrosion-resistant material is selected from cross-linked polyethylene, polyvinylidene fluoride or a combination thereof.

[0023] Preferably, the segmented cooling pipe consists of four sections, each section is equipped with an independent PID controller for adjusting the temperature and flow rate of the cooling water. The control range is from 10°C to 25°C, and the flow rate range is from 200mL / min to 500mL / min to meet the requirements of pipes with different extrusion speeds and thicknesses.

[0024] Preferably, the visual inspection system comprises:

[0025] At least two high-resolution industrial cameras, each with a resolution of at least 1920x1080 pixels;

[0026] Equipped with high-speed image processing software, which can process at least 500 frames per second in real time and automatically detect surface defects of 0.1mm to 0.5mm;

[0027] The ultrasonic thickness measuring device consists of four measuring points, each of which can independently provide wall thickness data accurate to 0.01 mm, and the data update frequency is 100 times per second to provide high-precision wall thickness control.

[0028] Preferably, the three-layer co-extrusion head is equipped with an independent heating belt with a temperature control accuracy of ±1°C and an electronic flow meter with a flow control accuracy of ±0.5%, which is used to accurately control the temperature and extrusion rate of each layer of material. Each layer of the extrusion head is also equipped with a pressure sensor with a measurement accuracy of ±2kPa to monitor and adjust the material flow pressure during the extrusion process to ensure the quality of the product and the interlayer adhesion.

[0029] Preferably, the plasma processing device includes a variable power plasma generator with a power range from 100 watts to 200 watts, which can automatically adjust the power and processing time, and the adjustable time range is from 1 second to 3 seconds to adapt to different pipe diameters and material types. The plasma processing device is equipped with temperature and ionization density sensors to monitor the state of the processing environment in real time to ensure the consistency and repeatability of the processing effect.

[0030] The present invention provides a process for preparing an ultra-flexible fixed-length pipe for gas, which has the following beneficial effects:

[0031] 1. The present invention significantly enhances the mechanical strength, wear resistance and chemical corrosion resistance of the pipe by mixing high-density polyethylene with nano-clay and nano-silicon dioxide. The use of this nano-composite material effectively solves the problem of easy damage to the pipe in harsh environments and improves the service life and safety of the pipe.

[0032] 2. The present invention ensures uniform processing of the composite material throughout the extrusion process by equipping the extruder with a precisely controlled three-layer co-extrusion head and an independent heating belt, as well as implementing precise temperature control. This control strategy solves the problem of inconsistent material properties caused by temperature fluctuations or uneven heating, and ensures high quality and consistency of the product.

[0033] 3. The present invention adopts segmented cooling pipelines, each segment is equipped with an independent PID controller, which can accurately adjust the temperature and flow rate of cooling water to meet the needs of different extrusion speeds and thicknesses. This fine control effectively reduces internal stress and physical deformation, and solves the problem of product deformation and performance degradation caused by uneven cooling in traditional production processes.

[0034] 4. The present invention realizes real-time quality monitoring and automatic parameter adjustment by using an online intelligent detection system implemented by a high-resolution industrial camera and ultrasonic thickness measuring equipment. This automated production mode significantly improves production efficiency, reduces manual dependence, and ensures the quality consistency of each batch of products and the predictability of production.

[0035] 5. The plasma treatment technology of the present invention is optimized for different pipe diameters and material types through adjustable power and treatment time, significantly improving the adhesion and anti-corrosion performance of the pipe surface. The application of this technology solves the problem of poor adhesion of traditional pipes during coating and surface treatment, and improves the durability and protective effect of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Process flow chart for preparing ultra-flexible cut-to-length pipes for gas. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example:

[0039] Please see attached Figure 1 .

[0040] Example

[0041] Example 1: Preparation of ultra-flexible fixed-length pipe for domestic gas transportation

[0042] Steps: a) Mix high-density polyethylene with nanomaterials (3% nanoclay and 1% nanosilica). b) Pre-mix the raw materials in a high-shear mixer at a speed of 5000rpm, and the temperature of the twin-screw extruder is set to 220℃. c) Use an extruder equipped with a three-layer co-extrusion head to extrude at a temperature of 220℃ to form a three-layer structural pipe. d) The outer layer uses aging-resistant polyethylene containing UV stabilizer, the middle layer is a nano-composite reinforced material, and the inner layer is a cross-linked polyethylene. e) The cooling channel is controlled in four stages, the temperature gradually decreases from 15℃ to 10℃, and the flow rate is maintained at 300mL / min. f) The stretching ratio is set to 1.2, and the laser cutting technology with an accuracy of ±0.1mm is used for fixed-length cutting. g) The surface treatment uses 150-watt plasma treatment for a duration of 2 seconds. h) Quality monitoring is carried out using a visual inspection system and an ultrasonic thickness measurement device.

[0043] Summary: The pipe in this embodiment has good aging resistance and mechanical properties, is suitable for household gas transportation, and ensures long-term durability and safety.

[0044] Example 2: Preparation of high pressure-resistant ultra-flexible fixed-length pipe for industrial gas transportation

[0045] Steps: a) Mix high density polyethylene with 4% nano silica. b) Mix in high shear mixer at 6000rpm, twin screw extruder temperature at 225°C. c) Three-layer co-extruder at 230°C. d) Outer layer is polypropylene with UV stabilizer, middle layer is nanocomposite reinforcement, inner layer is polyvinylidene fluoride. e) Cooling pipe temperature drops from 25°C to 20°C, flow rate is 500mL / min. f) Stretch ratio 1.2, cut to length accuracy ±0.1mm. g) Plasma treatment set to 200 watts, treatment time 3 seconds. h) Quality monitoring uses vision system and ultrasonic thickness measurement.

[0046] Summary: Suitable for industrial gas transportation in high-pressure environments, especially in chemically corrosive environments, providing superior chemical stability and mechanical strength.

[0047] Example 3: Ageing-resistant ultra-flexible cut-to-length tube for extreme external environments

[0048] Steps: a) High density polyethylene mixed with 2% nano clay and 2% nano silica. b) Premixing at 4000rpm, twin screw extruder temperature 215℃. c) Three-layer co-extruder extrusion at 210℃. d) Special aging-resistant polymer for the outer layer, nano composite material for the middle layer, and cross-linked polyethylene for the inner layer. e) Cooling pipe temperature from 20℃ to 10℃ in stages, flow rate 200mL / min. f) Stretch ratio 1.2, cut-to-length accuracy ±0.1mm. g) Plasma treatment 150 watts, 1 second. h) Monitoring using high-resolution camera and ultrasonic thickness gauge.

[0049] Summary: Especially suitable for areas with harsh external environment, such as high UV radiation areas. The special aging-resistant material of the outer layer can effectively prevent damage caused by UV.

[0050] Example 4: Ultra-flexible pipe with high sanitation standards for gas transportation in hospitals

[0051] Steps: a) High density polyethylene mixed with 3% nano clay and 1% nano silica. b) Mixing at 5000rpm, twin screw extruder temperature 220℃. c) Extrusion at 225℃ using a three-layer co-extruder. d) The outer layer uses high density polyethylene with UV stabilizer, the middle layer is a nano composite material, and the inner layer is polyvinylidene fluoride. e) Cooling from 25℃ to 15℃, flow rate 250mL / min. f) Stretch ratio 1.2, cut to length accuracy ±0.1mm. g) Plasma treatment 200 watts, 2 seconds. h) Quality monitoring uses high-resolution industrial cameras and ultrasonic thickness measurement equipment.

[0052] Summary: It provides gas transmission pipes with high hygiene standards, suitable for use in medical environments, and the inner layer of polyvinylidene fluoride ensures the purity and safety of the gas.

[0053] Example 5: Ultra-flexible cut-to-length tube for cryogenic environments

[0054] Steps: a) High density polyethylene mixed with 4% nanoclay. b) Mixing in high shear mixer at 6000rpm, twin screw extruder temperature 215℃. c) Extrusion at 210℃ using a three-layer co-extruder. d) Outer layer using high density polyethylene, middle layer nanocomposite, inner layer cross-linked polyethylene. e) Cooling channel temperature from 10℃ to 5℃, minimum flow rate 200mL / min. f) Stretch ratio 1.2, cut to length accuracy ±0.1mm. g) Plasma treatment 150 watts, duration 1 second. h) Quality monitoring using vision system and ultrasonic thickness measurement equipment.

[0055] Summary: It is particularly suitable for low temperature environments, such as outdoor in winter or cold storage. The inner layer of cross-linked polyethylene ensures mechanical properties and chemical stability at low temperatures.

[0056] Summary:

[0057] These examples demonstrate the wide applicability of the present invention in different application scenarios, from household to industrial, medical and special environment applications, the present invention can provide superior mechanical properties, chemical corrosion resistance and high production efficiency. Through precise material control and advanced production technology, high-quality and high-performance ultra-flexible cut-to-length pipes for gas are prepared.

[0058] Comparative Experimental Design

[0059] In order to verify the advantages of the ultra-flexible cut-to-length pipe of the present invention over the traditional high-density polyethylene pipe in various properties, the following detailed comparative experiments will be conducted to measure the tensile strength, chemical corrosion resistance and UV resistance respectively.

[0060] Experimental Materials

[0061] Traditional high-density polyethylene pipe (without nanomaterials added)

[0062] The ultra-flexible fixed-length tube of the present invention (high-density polyethylene containing nanomaterials)

[0063] Experimental methods:

[0064] Tensile strength test:

[0065] Instrument: Standard tensile testing machine

[0066] Method: According to ASTM D638 standard, the test speed is 50 mm / min and the test temperature is 23°C.

[0067] Sample size: length 200mm, width 10mm, thickness according to the actual sample.

[0068] Chemical corrosion resistance test:

[0069] Equipment: Balance and sealed container

[0070] Method: Soak the sample in 10% hydrochloric acid solution for 72 hours, then take it out, rinse it, air-dry it and weigh it.

[0071] Calculation: Chemical resistance is expressed as a percentage change in weight.

[0072] UV resistance test:

[0073] Instrument: UV aging test chamber

[0074] Method: According to ASTM G154 standard, continuous exposure for 200 hours.

[0075] Evaluation: The color change after UV was evaluated by a color change rating system (1 is the best and 5 is the worst).

[0076] Experimental data record table:

[0077]

[0078] Experimental steps:

[0079] Prepare sample strips of the same size.

[0080] The tensile strength test was performed using a tensile testing machine and the maximum force before fracture was recorded.

[0081] The sample strip is immersed in a chemical solution and the weight change is recorded at regular intervals.

[0082] Place the sample strips into the UV aging test chamber, take them out after the set time, and observe and record the color change level.

[0083] Summarize all data and conduct comparative analysis.

[0084] Expected results of the experiment:

[0085] Tensile strength: It is expected that the ultra-flexible cut-to-length tube of the present invention will have a significantly higher tensile strength than conventional high-density polyethylene tubes due to the nano-reinforced material.

[0086] Chemical corrosion resistance: Due to the protective effect of nanomaterials, the chemical corrosion resistance of the pipe of the present invention is expected to be better than that of traditional pipes.

[0087] UV resistance: Since the outer layer contains a UV stabilizer, the UV resistance of the pipe of the present invention will be better than that of the traditional pipe without adding a UV stabilizer.

[0088] Experimental summary:

[0089] This comparative experiment will intuitively demonstrate the advantages of the ultra-flexible fixed-length pipe of the present invention over the traditional high-density polyethylene pipe in multiple key performance aspects. The effectiveness of the present invention can be proved by the experiment, which can provide strong support and reasons for the application of the new pipe in the field of gas transportation.

[0090] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for preparing ultra-flexible fixed-length pipes for gas, characterized in that: The following steps are involved: a) Providing raw materials: mixing high-density polyethylene with nanomaterials; b) Pretreatment of composite materials: premixing the raw materials in a high shear mixer and fusing them at a constant temperature in a twin-screw extruder; c) Extrusion molding: The extruder is equipped with a precisely controlled three-layer co-extrusion head to extrude the composite material at a temperature range of 210°C to 230°C to form a multi-layer structure pipe; d) Multi-layer co-extrusion structure: the outer layer uses an aging-resistant polymer containing UV stabilizer, the middle layer is a nano-composite reinforcement material, and the inner layer is a chemical corrosion-resistant material; e) Intelligent cooling system: through the segmented cooling pipe equipped with temperature and flow rate sensors, the state of the cooling medium is monitored and adjusted in real time to ensure the uniformity of material properties; f) Synchronous stretching and cutting to length: The stretching ratio is adjusted to 1.2 using a servo motor-controlled stretching device, followed by cutting to length using laser cutting technology with an accuracy of ±0.1 mm; g) Surface treatment and functionalization: plasma treatment with a power of 150 watts and a treatment time of 1-3 seconds to improve the adhesion of the coating; h) Online intelligent detection: Using visual inspection system and ultrasonic thickness measurement equipment, set the sampling frequency to 200 times per second, real-time monitoring and automatic adjustment of production parameters based on the results.

2. The process for preparing an ultra-flexible fixed-length pipe for gas according to claim 1, characterized in that: The nanometer material comprises nanometer clay and nanometer silicon dioxide, and the total proportion of the nanometer material is 2% to 4% of the total weight of the substrate.

3. The process for preparing an ultra-flexible fixed-length pipe for gas according to claim 1, characterized in that: The rotation speed of the high shear mixer is 4000 to 6000 revolutions per minute; the temperature of the twin-screw extruder is controlled at 215° C. to 225° C.

4. The process for preparing an ultra-flexible fixed-length pipe for gas according to claim 1, characterized in that: The multi-layer co-extrusion structure specifically has an outer layer thickness of 0.5 mm to 1 mm, a middle layer thickness of 2 mm to 3 mm, and an inner layer thickness of 0.5 mm to 1 mm.

5. The process for preparing an ultra-flexible fixed-length pipe for gas according to claim 1, characterized in that: The aging-resistant polymer is selected from high-density polyethylene, polypropylene or a combination thereof; the nano-composite reinforcing material is selected from nano-clay, nano-silicon dioxide or a combination thereof; the chemical corrosion-resistant material is selected from cross-linked polyethylene, polyvinylidene fluoride or a combination thereof.

6. The process for preparing an ultra-flexible fixed-length pipe for gas according to claim 1, characterized in that: The segmented cooling pipeline consists of four sections, each section is equipped with an independent PID controller for adjusting the temperature and flow rate of cooling water. The control range is from 10°C to 25°C, and the flow rate range is from 200mL / min to 500mL / min to meet the requirements of pipes with different extrusion speeds and thicknesses.

7. The process for preparing an ultra-flexible fixed-length pipe for gas according to claim 1, characterized in that: The visual inspection system comprises: At least two high-resolution industrial cameras, each with a resolution of at least 1920x1080 pixels; Equipped with high-speed image processing software, which can process at least 500 frames per second in real time and automatically detect surface defects of 0.1mm to 0.5mm; The ultrasonic thickness measuring device consists of four measuring points, each of which can independently provide wall thickness data accurate to 0.01 mm, and the data update frequency is 100 times per second to provide high-precision wall thickness control.

8. The process for preparing an ultra-flexible fixed-length pipe for gas according to claim 1, characterized in that: The three-layer co-extrusion head is equipped with an independent heating belt with a temperature control accuracy of ±1°C and an electronic flow meter with a flow control accuracy of ±0.5%, which is used to accurately control the temperature and extrusion rate of each layer of material. Each layer of the extrusion head is also equipped with a pressure sensor with a measurement accuracy of ±2kPa to monitor and adjust the material flow pressure during the extrusion process to ensure the quality of the product and the interlayer adhesion.

9. The process for preparing an ultra-flexible fixed-length pipe for gas according to claim 1, characterized in that: The plasma processing device includes a variable power plasma generator with a power range from 100 watts to 200 watts. The power and processing time can be automatically adjusted. The adjustable time range is from 1 second to 3 seconds to adapt to different pipe diameters and material types. The plasma processing device is equipped with temperature and ionization density sensors to monitor the status of the processing environment in real time.

Citation Information

Cited By

  • Weather-resistant photovoltaic pipe and forming method thereof

    CN119505423A