Preparation method of carbon fiber paper for gas diffusion layer of fuel cell and carbon fiber paper for gas diffusion layer

By forming a preoxidized nanofiber membrane on the carbon fiber felt and performing hot-pressed carbonization graphitization treatment, carbon fiber paper with excellent pore structure was prepared, which solved the problem of insufficient pore structure design in the traditional carbon paper preparation process and improved fuel cell gas Performance and lifetime of the diffusion layer.

CN119017800AInactive Publication Date: 2024-11-26SHANGHAI JAZZ MATERIAL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411217559.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The traditional carbon paper preparation process lacks a pore structure design for specific needs in structure, which affects the overall performance of the fuel cell, especially the porosity and pore size distribution of the gas diffusion layer are not suitable, affecting the transmission efficiency of electrons, gas and water.

Method used

By forming a preoxidized nanofiber membrane on the carbon fiber felt, forming a composite carbon fiber felt stack, and carbon fiber paper with excellent pore structure was prepared by hot pressing and graphitization of carbon fiber, and its pore structure was finely regulated.

Benefits of technology

The performance improvement of the gas diffusion layer of the fuel cell is achieved, the transmission efficiency of electrons, gas and water is improved, and the life and stability of the fuel cell is extended.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of carbon fiber paper for a gas diffusion layer of a fuel cell. The preparation method comprises the following steps: forming a pre-oxidized nanofiber membrane; placing the pre-oxidized nanofiber membrane on a carbon fiber felt laminated layer according to a preset total weight to form a composite carbon fiber felt laminated layer; forming carbon fiber hot-pressed paper based on the composite carbon fiber felt lamination; and performing carbonization and graphitization treatment on the carbon fiber hot-pressed paper to obtain the carbon fiber paper. The carbon fiber paper for the fuel cell gas diffusion layer with excellent performance can be obtained, and powerful material support is provided for development of the fuel cell technology. The invention also discloses the carbon fiber paper for the gas diffusion layer prepared by the method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fuel cells, and in particular to a carbon fiber paper for a fuel cell gas diffusion layer and a preparation method and application thereof. Background Art

[0002] With the increasing global awareness of environmental protection and the rapid growth of demand for sustainable energy, hydrogen energy, with its green and low-carbon characteristics and diversified application scenarios, is increasingly emerging and becoming one of the key media to promote the development of global energy transformation. In addition, the hydrogen energy industry has also been established as a key development direction for strategic emerging industries and future industries. This strategic positioning highlights the important role of hydrogen energy in my country's future energy transformation. As an important branch of hydrogen energy applications, proton exchange membrane fuel cells (PEMFC) have attracted widespread attention due to their high efficiency and environmental protection. In PEMFC, the gas diffusion layer (GDL) is a core component, and its performance directly affects the overall efficiency of the fuel cell. The GDL is located between the catalyst layer and the bipolar plate, and is mainly composed of a substrate layer and a microporous layer. Among them, the substrate layer uses carbon fiber paper as the main material. This material has excellent porosity and conductivity, and the pore diameters are mostly concentrated between 50 and 150 μm. In order to optimize the interfacial electrochemical performance and gas transmission efficiency, a microporous layer is added between the carbon paper and the catalytic layer as an intermediate transition layer. It is made of a mixture of polytetrafluoroethylene (PTFE) and carbon black, and the pore size range is usually between 10 and 50 μm. The microporous layer not only helps to improve the electrochemical performance, but also reserves gas transmission channels, forms a part of hydrophobic pores, effectively prevents flooding, and promotes the redistribution of gas and water to a certain extent, which is of great significance for enhancing battery stability and extending life. However, the traditional carbon paper preparation process has limitations. The conventional preparation process involves the steps of resin impregnation, hot pressing curing, and carbonization and graphitization of carbon fiber felt. The obtained carbon paper has uniform micron-level pores in structure and lacks pore structure design for specific needs. Summary of the invention

[0003] The purpose of the present invention is to address the deficiencies of the prior art and provide a proton exchange membrane fuel cell gas diffusion layer with suitable porosity and pore size distribution to ensure the transmission of electrons, gas and water, thereby improving the overall performance of the fuel cell.

[0004] In order to achieve the above technical objectives, some embodiments of the present invention provide a method for preparing carbon fiber paper for fuel cell gas diffusion layer, which includes the steps 1. A method for preparing carbon fiber paper for fuel cell gas diffusion layer, characterized in that it includes the steps of: forming a pre-oxidized nanofiber membrane; placing the pre-oxidized nanofiber membrane on a carbon fiber felt stack according to a predetermined total weight to form a composite carbon fiber felt stack; forming a carbon fiber hot-pressed paper based on the composite carbon fiber felt stack; and carbonizing and graphitizing the carbon fiber hot-pressed paper to obtain the carbon fiber paper.

[0005] In some embodiments, the formation of the pre-oxidized nanofiber membrane includes step S1: preparing a spinning solution containing thermoplastic phenolic resin, polyacrylonitrile, and an organic solvent; step S2: using the spinning solution to spin on aluminum foil through an electrostatic spinning process to obtain a nanofiber membrane; and step S3: pre-oxidizing the nanofiber membrane to obtain the pre-oxidized nanofiber membrane; wherein, step S1 is to dissolve polyacrylonitrile in an organic solvent, heat and dissolve it at 40-60°C for 2-24 hours, and stir to form a homogeneous electrospinning solution; wherein the mass percentage of polyacrylonitrile is 15%; wherein, the organic solution is N, N-dimethylformamide (DMF) or N, N-dimethylacetamide (DMAc); The molecular weight of the thermoplastic phenolic resin is above 1000; the molecular weight of the polyacrylonitrile can be 50,000, 80,000, 150,000, or 200,000; or the step S1 is to dissolve the polyacrylonitrile and the thermoplastic phenolic resin in an organic solvent, heat at 40-60°C, stir and dissolve for 2-24 hours, and form a homogeneous electrospinning solution; wherein the mass percentage of the thermoplastic phenolic resin is 3%-8%; the mass percentage of the polyacrylonitrile is 7-12%; wherein the organic solution is N,N~dimethylformamide (DMF) or N,N~dimethylacetamide (DMAc); the molecular weight of the thermoplastic phenolic resin is above 1000; the molecular weight of the polyacrylonitrile is 50,000, 80,000, 150,000, or 200,000.

[0006] In some embodiments, the formation of a pre-oxidized nanofiber membrane includes step S1: preparing a spinning solution containing thermoplastic phenolic resin, polyacrylonitrile, and an organic solvent; step S2: using the spinning solution to spin on aluminum foil through an electrospinning process to obtain a nanofiber membrane; and step S3: pre-oxidizing the nanofiber membrane to obtain the pre-oxidized nanofiber membrane; wherein, step S1 is to dissolve polyacrylonitrile in an organic solvent, heat it at 40~60°C, and stir and dissolve it for 2~24 hours to form a homogeneous electrospinning solution; wherein the mass percentage of the thermoplastic phenolic resin is 1%~8%; the mass percentage of polyacrylonitrile is 7~14%; wherein the organic solution is N,N~dimethylformamide (DMF) or N,N~dimethylacetamide (DMAc); the molecular weight of the thermoplastic phenolic resin is above 1000; the molecular weight of the polyacrylonitrile is 50,000, 80,000, 150,000 or 200,000.

[0007] In some embodiments, the single tube advancement speed in the electrospinning process in step S2 is 0.1-1.5 mL / h, the high-voltage electrostatic voltage is 5-25 KV, and the spinning distance is controlled at 10-20 cm.

[0008] In some embodiments, the pre-oxidation heat treatment temperature in step S3 is 200-350° C., the heating rate is 0.5-20° C. / min, and the pre-oxidation heat treatment time is 0.5-3 h.

[0009] In some embodiments, the formation of the composite carbon fiber felt further includes step S4: cutting the carbon fiber felt into a preset size and placing the carbon fiber felt in overlapping layers according to a preset total grammage to form a carbon fiber felt laminate; and step S5: cutting the pre-oxidation heat-treated nanofiber membrane into a preset size and laminating it on the carbon fiber felt laminate to obtain a composite carbon fiber felt; the grammage range of the carbon fiber felt in step S4 is controlled to be 10~30 g / m 2 The total weight of the carbon fiber felt laminate is between 40 and 60 g / m 2 The mass of the pre-oxidized nanofiber membrane in step S5 is 1 to 3 times that of the carbon fiber felt laminate.

[0010] In some embodiments, forming the carbon fiber hot-pressed paper may include step S6: immersing the composite layer carbon fiber felt in an aqueous solution of a thermosetting phenolic resin, taking it out and pre-curing it in an oven to obtain preformed paper; and step S7: hot-pressing the preformed paper on a flat vulcanizer to obtain carbon fiber hot-pressed paper.

[0011] In some embodiments, the resin solution in step S6 includes an aqueous solution of a thermosetting water-soluble phenolic resin; the concentration of the thermosetting water-soluble phenolic resin in the aqueous solution is 10-30wt%, and the immersion time is 0.5-3h; the hot pressing pressure in step S7 is 5-11MPa, the hot pressing temperature is 150-350°C, and the hot pressing time is 0.5-12h.

[0012] In some embodiments, the carbon fiber hot-pressed paper is carbonized and graphitized, including step S8: carbonizing and graphitizing the carbon fiber hot-pressed paper at a preset temperature and a protective atmosphere to obtain the carbon fiber paper; in step S8, the carbonization temperature is 900-1200°C, the heating rate is 5-10°C / min, and the heat preservation is 2-4 h; the graphitization temperature is 2000-2500°C, the heating rate is 5-10°C / min, and the heat preservation is 2-6 h.

[0013] Some embodiments of the present application provide carbon fiber paper for a gas diffusion layer, which is prepared by any of the methods described above.

[0014] The preparation method proposed in this application introduces a nanofiber membrane on one side of the carbon paper to achieve fine control of its pore structure. Through this innovative preparation method, the present invention can obtain carbon fiber paper for fuel cell gas diffusion layer with excellent performance, providing strong material support for the development of fuel cell technology. DETAILED DESCRIPTION

[0015] The present invention is further described in detail below through preferred embodiments. The following embodiments can enable those skilled in the art to understand the present invention more comprehensively, but do not limit the present invention in any way.

[0016] Unless otherwise defined, the unit symbols used in this document are g for gram, °C for degree Celsius, h for hour, kV for kilovolt, cm for centimeter, mL / min for milliliter per minute, and g / m 2 Indicates grams per square meter; cm 2 represents square centimeters; wt% represents weight percentage; ℃ / min represents degrees Celsius per minute; μm represents micrometers; MPa represents megapascals; mΩ·cm 2 It represents milliohm-cm2.

[0017] Some embodiments of the present application provide a method for preparing carbon fiber paper for a fuel cell gas diffusion layer, which includes forming a pre-oxidized nanofiber membrane; placing the pre-oxidized nanofiber membrane on a carbon fiber felt stack according to a predetermined total weight to form a composite carbon fiber felt stack; then forming a carbon fiber hot-pressed paper based on the composite carbon fiber felt stack; and finally carbonizing and graphitizing the carbon fiber hot-pressed paper to obtain the carbon fiber paper.

[0018] Among them, the formation of the pre-oxidized nanofiber membrane may include step S1: preparing a spinning solution containing thermoplastic phenolic resin, polyacrylonitrile, and an organic solvent; step S2: using the spinning solution to spin on aluminum foil through an electrospinning process to obtain a nanofiber membrane; and step S3: performing a pre-oxidation heat treatment on the nanofiber membrane to obtain the pre-oxidized nanofiber membrane.

[0019] Further, the step S1 is to dissolve the thermoplastic phenolic resin and polyacrylonitrile in an organic solvent, and stir and dissolve them at 40-60°C for 2-24 hours to form a homogeneous electrospinning solution; wherein the mass percentage of the thermoplastic phenolic resin is 0%-8%, preferably 3%-7%; the mass percentage of polyacrylonitrile is 7-15%, preferably 8-12%. The organic solvent is N, N~ dimethylformamide (DMF) or N, N~ dimethylacetamide (DMAc); the molecular weight of the thermoplastic phenolic resin is above 1000; the molecular weight of the polyacrylonitrile can be 50,000, 80,000, 150,000, 200,000, preferably 80,000 and 150,000.

[0020] Furthermore, in step S2, the single tube advancement speed during the electrospinning process is 0.1-1.5 mL / h, the high voltage electrostatic voltage is 5-25 KV, and the spinning distance is controlled at 10-20 cm.

[0021] Further, in step S3, the pre-oxidation heat treatment temperature is 200-350° C., the heating rate is 0.5-20° C. / min, and the pre-oxidation heat treatment time is 0.5-3 h.

[0022] The formation of the composite carbon fiber felt may further include step S4: cutting the carbon fiber felt into a preset size and placing the carbon fiber felt in overlapping layers according to a preset total gram to form a carbon fiber felt laminate; and step S5: cutting the pre-oxidation heat-treated nanofiber membrane into a preset size and laminating it on the carbon fiber felt laminate to obtain a composite carbon fiber felt; Further, the weight range of the carbon fiber felt in step S4 is controlled to be 10-30 g / m 2 The total weight of the carbon fiber felt laminate is between 40 and 60 g / m 2 between.

[0023] Furthermore, the mass of the pre-oxidized nanofiber membrane in step S5 is 1 to 5 times that of the carbon fiber felt laminate.

[0024] Among them, forming the carbon fiber hot-pressed paper may include step S6: immersing the composite layer carbon fiber felt in an aqueous solution of a thermosetting phenolic resin, taking it out and pre-curing it in an oven for a period of time to obtain preformed paper; and step S7: hot-pressing the preformed paper on a flat vulcanizer to obtain carbon fiber hot-pressed paper.

[0025] Furthermore, the resin solution in step S6 comprises an aqueous solution of a thermosetting water-soluble phenolic resin; the concentration of the thermosetting water-soluble phenolic resin in the resin solution is 10 to 30 wt %, and the immersion time is 0.5 to 3 h.

[0026] Furthermore, in step S7, the hot pressing pressure is 5-11 MPa, the hot pressing temperature is 150-350° C., and the hot pressing time is 0.5-12 h.

[0027] The carbon fiber hot-pressed paper is subjected to carbonization and graphitization treatment, including step S8: carbonizing and graphitizing the carbon fiber hot-pressed paper under a preset temperature and a protective atmosphere to obtain the carbon fiber paper.

[0028] Furthermore, in step S8, the carbonization temperature is 900-1200°C, the heating rate is 5-10°C / min, and the temperature is kept for 2-4 hours. The graphitization temperature is 2000-2500°C, the heating rate is 5-10°C / min, and the temperature is kept for 2-6 hours.

[0029] Example 1 1.5 g of polyacrylonitrile powder was weighed and dissolved in 8.5 g of N, N-dimethylformamide (DMF) solvent, and stirred and dissolved at 50 °C for 6 h to form a homogeneous electrospinning solution; the prepared electrospinning solution was electrospun on the surface of aluminum foil to form a layer of nanofiber membrane, wherein the electrospinning voltage was 15 kV, the vertical distance from the needle tip to the support layer was 15 cm, the spinning rate was 1 mL / min, and the spinning temperature was 20 °C; after the spinning was completed, the removed fiber membrane was placed in an oven at 250 °C for pre-oxidation for 2 h to obtain a pre-oxidized fiber membrane; 10 g / m 2 The carbon fiber felt is cut into 10×10 cm 2 And the total weight is 50 g / m 2The carbon fiber felt and the pre-oxidized fiber membrane are stacked in a mass ratio of 1:1, with the pre-oxidized fiber membrane on the upper layer. Water-soluble phenolic resin and deionized water were prepared into resin solutions with a concentration of 10 wt%, which were fully stirred for 30 min by a magnetic stirrer and then uniformly mixed as impregnation solutions; the laminated samples were immersed in the prepared 10 wt% resin solution for 30 min, and then pre-cured for 30 min by hanging drying after being taken out to obtain carbon fiber pre-cured paper; the carbon fiber pre-cured paper was placed in a customized mold by a laminated hot pressing method, and pressed for 10 h at a temperature of 290 ℃ and a pressure of 10 MPa to obtain carbon fiber hot-pressed paper; the carbon fiber hot-pressed paper was placed in a carbonization furnace, and carbonized at a temperature of 1000 ℃, a heating rate of 10 ℃ / min, and a heat preservation of 4 h under the protection of an inert atmosphere to obtain carbon fiber carbonized paper; then the carbon fiber carbonized paper was placed in a graphitization furnace, and under the protection of an inert atmosphere, the heating rate was 5 ℃ / min, and the highest temperature was 2000 ℃, and graphitization treatment was performed to obtain carbon fiber paper. The thickness of the carbon fiber paper prepared in Example 1 is 190 μm. The pore structure of the microporous layer of the sample is characterized by a mercury intrusion instrument. The test shows that the porosity of the sample is 72%, and the TP resistance value under a pressure of 1 MPa is only 12.8 mΩ·cm 2 .

[0030] Example 2 1.5 g of polyacrylonitrile powder was weighed and dissolved in 8.5 g of N, N-dimethylformamide (DMF) solvent, and stirred and dissolved at 50 °C for 6 h to form a homogeneous electrospinning solution; the prepared electrospinning solution was electrospun on the surface of aluminum foil to form a layer of nanofiber membrane, wherein the electrospinning voltage was 15 kV, the vertical distance from the needle tip to the support layer was 15 cm, the spinning rate was 1 mL / min, and the spinning temperature was 20 °C; after the spinning was completed, the removed fiber membrane was placed in an oven at 250 °C for pre-oxidation for 2 h to obtain a pre-oxidized fiber membrane; 10 g / m 2 The carbon fiber felt is cut into 10×10 cm 2 And the total weight is 50 g / m 2The carbon fiber felt and the pre-oxidized fiber membrane are stacked in a mass ratio of 2:1, with the pre-oxidized fiber membrane on the upper layer. Water-soluble phenolic resin and deionized water were prepared into resin solutions with a concentration of 10 wt%, which were fully stirred for 30 min by a magnetic stirrer and then uniformly mixed as impregnation solutions; the laminated samples were immersed in the prepared 10 wt% resin solution for 30 min, and then pre-cured for 30 min by hanging drying after being taken out to obtain carbon fiber pre-cured paper; the carbon fiber pre-cured paper was placed in a customized mold by a laminated hot pressing method, and pressed for 10 h at a temperature of 290 ℃ and a pressure of 10 MPa to obtain carbon fiber hot-pressed paper; the carbon fiber hot-pressed paper was placed in a carbonization furnace, and carbonized at a temperature of 1000 ℃, a heating rate of 10 ℃ / min, and a heat preservation of 4 h under the protection of an inert atmosphere to obtain carbon fiber carbonized paper; then the carbon fiber carbonized paper was placed in a graphitization furnace, and under the protection of an inert atmosphere, the heating rate was 5 ℃ / min, and the highest temperature was 2000 ℃, and graphitization treatment was performed to obtain carbon fiber paper. The thickness of the carbon fiber paper prepared in Example 2 is 260 μm. The pore structure of the microporous layer of the sample is characterized by a mercury intrusion instrument. The test shows that the porosity of the sample is 73%, and the TP resistance value under a pressure of 1 MPa is only 12.2 mΩ·cm 2 .

[0031] Example 3 0.7 g of polyacrylonitrile powder and 0.8 g of thermoplastic phenolic resin powder were weighed and dissolved in 8.5 g of N, N-dimethylformamide (DMF) solvent, and stirred and dissolved at 50 °C for 6 h to form a homogeneous electrospinning solution; the prepared electrospinning solution was electrospun on the surface of aluminum foil to form a layer of nanofiber membrane, wherein the electrospinning voltage was 15 kV, the vertical distance from the needle tip to the support layer was 15 cm, the spinning rate was 1 mL / min, and the spinning temperature was 20 °C; after the spinning was completed, the removed fiber membrane was placed in an oven at 250 °C for pre-oxidation for 2 h to obtain a pre-oxidized fiber membrane; 10 g / m 2 The carbon fiber felt is cut into 10×10 cm 2 And the total weight is 50 g / m 2The carbon fiber felt and the pre-oxidized fiber membrane are stacked in a mass ratio of 3:1, with the pre-oxidized fiber membrane on the upper layer. Water-soluble phenolic resin and deionized water were prepared into resin solutions with a concentration of 10 wt%, which were fully stirred for 30 min by a magnetic stirrer and then uniformly mixed as impregnation solutions; the laminated samples were immersed in the prepared 10 wt% resin solution for 30 min, and then pre-cured for 30 min by hanging drying after being taken out to obtain carbon fiber pre-cured paper; the carbon fiber pre-cured paper was placed in a customized mold by a laminated hot pressing method, and pressed for 10 h at a temperature of 290 ℃ and a pressure of 10 MPa to obtain carbon fiber hot-pressed paper; the carbon fiber hot-pressed paper was placed in a carbonization furnace, and carbonized at a temperature of 1000 ℃, a heating rate of 10 ℃ / min, and a heat preservation of 4 h under the protection of an inert atmosphere to obtain carbon fiber carbonized paper; then the carbon fiber carbonized paper was placed in a graphitization furnace, and under the protection of an inert atmosphere, the heating rate was 5 ℃ / min, and the highest temperature was 2000 ℃, and graphitization treatment was performed to obtain carbon fiber paper. The thickness of the carbon fiber paper prepared in Example 3 is 220 μm. The pore structure of the microporous layer of the sample is characterized by a mercury intrusion instrument. The test shows that the porosity of the sample is 75%, and the TP resistance value under a pressure of 1 MPa is only 13.2 mΩ·cm 2 .

[0032] Example 4 0.7 g of polyacrylonitrile powder and 0.8 g of thermoplastic phenolic resin powder were weighed and dissolved in 8.5 g of N, N-dimethylformamide (DMF) solvent, and stirred and dissolved at 50 °C for 6 h to form a homogeneous electrospinning solution; the prepared electrospinning solution was electrospun on the surface of aluminum foil to form a layer of nanofiber membrane, wherein the electrospinning voltage was 15 kV, the vertical distance from the needle tip to the support layer was 15 cm, the spinning rate was 1 mL / min, and the spinning temperature was 20 °C; after the spinning was completed, the removed fiber membrane was placed in an oven at 250 °C for pre-oxidation for 2 h to obtain a pre-oxidized fiber membrane; 10 g / m 2 The carbon fiber felt is cut into 10×10 cm 2 And the total weight is 50 g / m 2The carbon fiber felt and the pre-oxidized fiber membrane are stacked in a mass ratio of 1:1, with the pre-oxidized fiber membrane on the upper layer. Water-soluble phenolic resin and deionized water were prepared into resin solutions with a concentration of 10 wt%, which were fully stirred for 30 minutes by a magnetic stirrer and then evenly mixed as impregnation solutions; the laminated samples were immersed in the prepared 10 wt% resin solution for 30 minutes, and then pre-cured for 30 minutes by hanging drying after being taken out to obtain carbon fiber pre-cured paper; the carbon fiber pre-cured paper was placed in a customized mold by a laminated hot pressing method, and pressed for 10 h at a temperature of 290 ℃ and a pressure of 10 MPa to obtain carbon fiber hot-pressed paper; the carbon fiber hot-pressed paper was placed in a carbonization furnace, and carbonized at a temperature of 1000 ℃, a heating rate of 10 ℃ / min, and a heat preservation of 4 hours under the protection of an inert atmosphere to obtain carbon fiber carbonized paper; then the carbon fiber carbonized paper was placed in a graphitization furnace, and under the protection of an inert atmosphere, the heating rate was 5 ℃ / min, and the highest temperature was 2000 ℃, and graphitization treatment was performed to obtain carbon fiber paper. The thickness of the carbon fiber paper prepared in Example 4 is 180 μm. The pore structure of the microporous layer of the sample is characterized by a mercury intrusion instrument. The test shows that the porosity of the sample is 72.5%, and the TP resistance value under a pressure of 1 MPa is only 14.4 mΩ·cm 2 .

[0033] Example 5 1.2 g of polyacrylonitrile powder and 0.3 g of thermoplastic phenolic resin powder were weighed and dissolved in 8.5 g of N, N-dimethylformamide (DMF) solvent, and stirred and dissolved at 50 °C for 6 h to form a homogeneous electrospinning solution; the prepared electrospinning solution was electrospun on the surface of aluminum foil to form a layer of nanofiber membrane, wherein the electrospinning voltage was 15 kV, the vertical distance from the needle tip to the support layer was 15 cm, the spinning rate was 1 mL / min, and the spinning temperature was 20 °C; after the spinning was completed, the removed fiber membrane was placed in an oven at 280 °C for pre-oxidation for 1 h to obtain a pre-oxidized fiber membrane; 10 g / m 2 The carbon fiber felt is cut into 10×10 cm 2 And the total weight is 50 g / m 2The carbon fiber felt and the pre-oxidized fiber membrane are stacked in a mass ratio of 3:1, with the pre-oxidized fiber membrane on the upper layer. Water-soluble phenolic resin and deionized water were prepared into resin solutions with a concentration of 10 wt%, which were fully stirred for 30 minutes by a magnetic stirrer and then evenly mixed as impregnation solutions; the laminated samples were immersed in the prepared 10 wt% resin solution for 30 minutes, and then pre-cured for 30 minutes by hanging drying after being taken out to obtain carbon fiber pre-cured paper; the carbon fiber pre-cured paper was placed in a customized mold by a laminated hot pressing method, and pressed for 10 h at a temperature of 290 ℃ and a pressure of 10 MPa to obtain carbon fiber hot-pressed paper; the carbon fiber hot-pressed paper was placed in a carbonization furnace, and carbonized at a temperature of 1000 ℃, a heating rate of 10 ℃ / min, and a heat preservation of 4 hours under the protection of an inert atmosphere to obtain carbon fiber carbonized paper; then the carbon fiber carbonized paper was placed in a graphitization furnace, and under the protection of an inert atmosphere, the heating rate was 5 ℃ / min, and the highest temperature was 2000 ℃, and graphitization treatment was performed to obtain carbon fiber paper. The thickness of the carbon fiber paper prepared in Example 5 is 200 μm. The pore structure of the microporous layer of the sample is characterized by a mercury intrusion instrument. The test shows that the porosity of the sample is 71.2%, and the TP resistance value under a pressure of 1 MPa is only 13.7 mΩ·cm 2 .

[0034] In other embodiments, the mass percentage of the polyacrylonitrile powder and the thermoplastic phenolic resin powder can be other range combinations whose sum can reach 15%, for example, the mass percentage of the thermoplastic phenolic resin is 1%~8%; the mass percentage of polyacrylonitrile is 7~14%; specifically, it can include 0.8g of polyacrylonitrile powder and 0.7g of the thermoplastic phenolic resin powder; 0.9g of polyacrylonitrile powder and 0.6g of the thermoplastic phenolic resin powder; 1.0g of polyacrylonitrile powder and 0.5g of the thermoplastic phenolic resin powder; 1.1g of polyacrylonitrile powder and 0.4g of the thermoplastic phenolic resin powder; 1.2g of polyacrylonitrile powder and 0.3g of the thermoplastic phenolic resin powder; 1.3g of polyacrylonitrile powder and 0.2g of the thermoplastic phenolic resin powder; 1.4g of polyacrylonitrile powder and 0.1g of the thermoplastic phenolic resin powder.

[0035] Comparative Example 1 This comparative example does not use the electrospinning process. Take 10g / m2 of carbon fiber base paper, cut it into 10×10cm2 and stack it with a total weight of 50g / m2 to obtain multi-layer carbon fiber base paper; take water-soluble phenolic resin and deionized water to prepare a resin solution with a concentration of 10 wt%, stir it thoroughly for 30 minutes with a magnetic stirrer and evenly mix it as an impregnation solution; immerse the multi-layer carbon fiber base paper in the prepared 10 wt% resin solution for 30 minutes, take it out and pre-cure it in a suspended drying method for 30 minutes to obtain carbon fiber pre-cured paper; use the stacking hot pressing method to place the carbon fiber pre-cured paper in a customized mold, press it at a temperature of 150 ℃ and a pressure of 10 MPa for 1 h to obtain carbon fiber hot-pressed paper; put the carbon fiber hot-pressed paper into a carbonization furnace, and keep it at a temperature of 1000 ℃, a heating rate of 10 ℃ / min, and a heat preservation of 4 h for carbonization to obtain carbon fiber carbonized paper; then the carbon fiber carbonized paper is placed in a graphitization furnace, and under the protection of an inert atmosphere, the heating rate is 5 ° C / min, the maximum temperature is 2000 ° C, and graphitization treatment is performed to obtain carbon fiber paper. The thickness of the carbon fiber paper prepared in Example 1 is 200 μm, and the pore structure of the microporous layer of the sample is characterized by a mercury intrusion instrument. The test shows that the porosity of the sample is 81.10%, and the TP resistance value under a pressure of 1 MPa is only 16.2 mΩ·cm2.

Claims

1. A method for preparing carbon fiber paper for a fuel cell gas diffusion layer, The method is characterized in that it comprises the steps of: forming a pre-oxidized nanofiber membrane; Placing the pre-oxidized nanofiber membrane on the carbon fiber felt laminate according to a predetermined total weight to form a composite carbon fiber felt laminate; forming carbon fiber hot-pressed paper based on the composite carbon fiber felt stack; as well as The carbon fiber hot-pressed paper is subjected to carbonization and graphitization treatment to obtain the carbon fiber paper.

2. The preparation method according to claim 1, characterized in that: The method for forming the pre-oxidized nanofiber membrane comprises step S1: preparing a spinning solution containing thermoplastic phenolic resin, polyacrylonitrile and an organic solvent; step S2: using the spinning solution to spin on aluminum foil paper through an electrostatic spinning process to obtain a nanofiber membrane; And step S3: pre-oxidizing and heat-treating the nanofiber membrane to obtain the pre-oxidized nanofiber membrane; wherein, step S1 is to dissolve polyacrylonitrile in an organic solvent, and stir and dissolve it at 40-60°C for 2-24 hours to form a homogeneous electrospinning solution; wherein the mass percentage of polyacrylonitrile is 15%; wherein, the organic solvent is N,N~dimethylformamide (DMF) or N,N~dimethylacetamide (DMAc); the molecular weight of the thermoplastic phenolic resin is above 1000; the molecular weight of the polyacrylonitrile can be 50,000, 80,000, 150,000, 200,000; or the step S1 is to dissolve polyacrylonitrile and thermoplastic phenolic resin in an organic solvent, and stir and dissolve them at 40-60°C for 2-24 hours to form a homogeneous electrospinning solution; wherein the mass percentage of thermoplastic phenolic resin is 3%-8%; the mass percentage of polyacrylonitrile is 7-12%; wherein the organic solvent is N,N-dimethylformamide (DMF) or N,N-dimethylacetamide (DMAc); the molecular weight of the thermoplastic phenolic resin is above 1000; the molecular weight of the polyacrylonitrile is 50,000, 80,000, 150,000 or 200,000.

3. The preparation method according to claim 1, characterized in that: The method for forming the pre-oxidized nanofiber membrane comprises step S1: preparing a spinning solution containing thermoplastic phenolic resin, polyacrylonitrile and an organic solvent; step S2: using the spinning solution to spin on aluminum foil paper through an electrostatic spinning process to obtain a nanofiber membrane; And step S3: pre-oxidation heat treatment of the nanofiber membrane to obtain the pre-oxidized nanofiber membrane; wherein, the step S1 is to dissolve polyacrylonitrile in an organic solvent, heat at 40-60°C and stir to dissolve for 2-24 hours to form a homogeneous electrospinning solution; wherein the mass percentage of thermoplastic phenolic resin is 1%-8%; the mass percentage of polyacrylonitrile is 7-14%; wherein the organic solution is N,N~dimethylformamide (DMF) or N,N~dimethylacetamide (DMAc); the molecular weight of the thermoplastic phenolic resin is above 1000; the molecular weight of the polyacrylonitrile is 50,000, 80,000, 150,000 or 200,000.

4. The method for preparing carbon fiber paper for fuel cell gas diffusion layer according to claim 2 or 3, characterized in that: In the electrospinning process in step S2, the single tube advancing speed is 0.1-1.5 mL / h, the high voltage electrostatic voltage is 5-25 KV, and the spinning distance is controlled at 10-20 cm.

5. The method for preparing carbon fiber paper for fuel cell gas diffusion layer according to claim 2 or 3, characterized in that: The pre-oxidation heat treatment temperature in step S3 is 200-350° C., the heating rate is 0.5-20° C. / min, and the pre-oxidation heat treatment time is 0.5-3 h.

6. The method for preparing carbon fiber paper for fuel cell gas diffusion layer according to claim 1, characterized in that: The formation of the composite carbon fiber felt further includes step S4: cutting the carbon fiber felt into a preset size and placing the carbon fiber felt in overlapping layers according to a preset total grammage to form a carbon fiber felt laminate; and step S5: cutting the pre-oxidation heat-treated nanofiber membrane into a preset size and laminating it on the carbon fiber felt laminate to obtain a composite carbon fiber felt; the grammage range of the carbon fiber felt in step S4 is controlled to be 10~30 g / m 2 The total weight of the carbon fiber felt laminate is between 40 and 60 g / m 2 The mass of the pre-oxidized nanofiber membrane in step S5 is 1 to 3 times that of the carbon fiber felt laminate.

7. The preparation method according to claim 1, characterized in that: Forming the carbon fiber hot-pressed paper may include step S6: immersing the composite layer carbon fiber felt in an aqueous solution of a thermosetting phenolic resin, taking it out and pre-curing it in an oven to obtain preformed paper; and step S7: hot-pressing the preformed paper on a flat vulcanizer to obtain carbon fiber hot-pressed paper.

8. The method for preparing carbon fiber paper for fuel cell gas diffusion layer according to claim 7, characterized in that: The resin solution in step S6 includes an aqueous solution of a thermosetting water-soluble phenolic resin; the concentration of the thermosetting water-soluble phenolic resin in the aqueous solution is 10-30wt%, and the impregnation time is 0.5-3h; the hot pressing pressure in step S7 is 5-11MPa, the hot pressing temperature is 150-350°C, and the hot pressing time is 0.5-12h.

9. The method for preparing carbon fiber paper for fuel cell gas diffusion layer according to claim 8, characterized in that: The carbon fiber hot-pressed paper is carbonized and graphitized, comprising step S8: carbonizing and graphitizing the carbon fiber hot-pressed paper at a preset temperature and a protective atmosphere to obtain the carbon fiber paper; in step S8, the carbonization temperature is 900-1200°C, the heating rate is 5-10°C / min, and the heat preservation is 2-4 hours; the graphitization temperature is 2000-2500°C, the heating rate is 5-10°C / min, and the heat preservation is 2-6 hours.

10. A carbon fiber paper for a gas diffusion layer, characterized in that: The gas diffusion layer is prepared by the method for preparing carbon fiber paper for fuel cell gas diffusion layer according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • A phenolic resin modified polyacrylonitrile precursor fiber and its preparation method

    CN102277644A

  • Hydrophobic modified carbon fiber paper as well as preparation method and application thereof

    CN115881983A

  • Carbon fiber paper as well as preparation method and application thereof

    CN116479545A

  • Carbon fiber paper and porous carbon electrode base material for fuel cells

    JP2004259711A

  • Fuel cell, carbon composite structure, and method of manufacturing the same

    JP2014098218A