Casting CPE (Chlorinated Polyethylene) cooking-resistant film and preparation method thereof

By using cast CPE film in a cooking resistant bag, combining specific ratios of HDPE, C6-LLDPE, C4-LLDPE and modified heat seals, as well as plasma-modified ultra-high molecular weight polyethylene fibers and modified nanowater Talc solves the problem of easy breakage and delamination of cooking bags during high temperature steaming, improves heat sealing strength and barrier properties, and extends the shelf life.

CN119017804APending Publication Date: 2024-11-26FUJIAN LIBANG PACKAGING CO LTD

Patent Information

Application Number
CN202411001688.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing steam-resistant cooking bags are easy to open and break when steaming at high temperature, and the composite bonding film layer is easily delaminated and peeled off after steaming, resulting in plastic contamination and difficulty in recycling.

Method used

Using cast CPE cooking-resistant film, including corona layer, intermediate layer and heat sealing layer, the tensile strength, impact resistance and Heat seal strength, plasma modified ultra-high molecular weight polyethylene fibers and modified nanohydrotalcite improve barrier properties and heat seal connection fastness.

Benefits of technology

It improves the heat seal strength and tear resistance of high-temperature cooking resistance, reduces the breakage rate, ensures the flat appearance and durability of the film, extends the shelf life of the packaging content, and improves the connection stability of the heat seal layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the field of high polymer materials, and particularly discloses a casting CPE (Chlorinated Polyethylene) cooking-resistant film and a preparation method thereof. The casting CPE cooking-resistant film comprises a corona layer, a middle layer and a heat sealing layer which are in contact with one another in sequence, and the corona layer comprises the following raw materials in percentage by weight: 55-60% of HDPE, 37-42% of C6-LLDPE and the balance of a processing aid; the middle layer is prepared from the following raw materials in percentage by weight: 60 to 65 percent of HDPE (High-Density Polyethylene), 27 to 30 percent of C6-LLDPE (C6-Linear Low Density Polyethylene) and 8 to 10 percent of C4-LLDPE; and the heat sealing layer comprises the following raw materials in percentage by weight: 50-55% of HDPE, 25-30% of C6-LLDPE, 13-15% of a modified heat sealing material and the balance of a processing aid. The cooking-resistant composite film has better heat sealing strength, is not easy to burst after being cooked, can resist high-temperature cooking at 121 DEG C, and has good barrier property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer materials, and more specifically, to a cast CPE cooking-resistant film and a preparation method thereof. Background Art

[0002] Retort bags, also known as soft cans, refer to composite films that can package food and withstand 121°C steam heating and sterilization. Compared with traditional metal canned containers, retort bags have the following advantages: First, the raw materials of retort bags are cheaper than metal plates, and their production process and processing equipment are relatively simple, so the manufacturing cost of retort bags is low; second, retort bags are thinner and can quickly reach the sterilization temperature, which not only reduces the sterilization energy consumption, but also preserves the original taste of the packaged food as much as possible; finally, retort bags are light and easy for consumers to carry. Therefore, in recent years, the market for retort bags has continued to expand, and is even expected to replace traditional metal packaging materials in some areas.

[0003] In the prior art, high-temperature retort bags are generally composite layers, and their basic structure is, from the outside to the inside, in the order of: surface layer, middle layer, heat-sealing layer, and different substrates are bonded together with adhesives. Since retort bags are made of multiple layers of different substrates bonded together, the manufacturing process is very complicated. Improper selection of adhesives, improper dosage, or bonding errors, insufficient pressure or temperature of the composite rollers may cause the retort bags to easily bubble, wrinkle, deform, and other production defects. In addition, the composite bonding film layer of the retort bag is also prone to delamination or breakage after retorting, and the retort bag cannot be recycled, which in turn causes plastic pollution.

[0004] In the prior art, a Chinese invention patent document with application number CN2021105212001 discloses a PE film that can withstand high-temperature cooking at 121°C, which is co-extruded by a corona layer, an intermediate layer and a heat-sealing layer; the corona layer material is 20-50wt% of bimodal metallocene medium-density polyethylene and 50-80wt% of high-density polyethylene; the intermediate layer material is bimodal metallocene medium-density polyethylene and / or high-density polyethylene; the heat-sealing layer material is 50-70wt% of bimodal metallocene medium-density polyethylene and 30-50wt% of high-density polyethylene.

[0005] After the above-mentioned retort-resistant film is made into a bag, it can maintain good stress cracking resistance during high-temperature retort. However, during the retort process, the retort bag is easily opened due to increased back pressure, and the bag breakage rate is high. Summary of the invention

[0006] In order to increase the heat sealing strength of the cooking bag and improve the high temperature cooking resistance, the present application provides a cast CPE cooking resistant film and a preparation method thereof.

[0007] In the first aspect, the present application provides a cast CPE cooking-resistant film, which adopts the following technical solution: A cast CPE cooking-resistant film comprises a corona layer, an intermediate layer and a heat-sealing layer which are in contact with each other in sequence, wherein the corona layer comprises the following raw materials in weight percentage: 55-60% HDPE, 37-42% C6-LLDPE, and the balance is a processing aid; The middle layer comprises the following raw materials in weight percentage: HDPE 60-65%, C6-LLDPE 27-30%, C4-LLDPE 8-10%; The heat sealing layer comprises the following raw materials in percentage by weight: 50-55% of HDPE, 25-30% of C6-LLDPE, 13-15% of modified heat sealing material, and the remainder is processing aid.

[0008] By adopting the above technical scheme, C6-LLDPE is polymerized by ethylene and a small amount of high-grade alpha olefins (such as 1-hexene C6) under the action of a catalyst, and has higher tensile strength, impact resistance, tear resistance and puncture resistance. Therefore, C6-LLDPE is added to the corona layer, the middle layer and the heat-sealing layer, which can effectively improve the tensile resistance of the composite film under high-temperature cooking, so that the composite film is not easy to burst or wrinkle under high temperature and high pressure, and has a relatively smooth appearance. C4-LLDPE is polymerized by ethylene and a small amount of high-grade alpha olefins (such as 1-butene, 1-hexene, 1-octene, etc.) under the action of a catalyst, and has lower density and crystallinity, but has higher heat resistance and cold resistance, and has a high surface gloss. Because of its linear structure, LLDPE molecules are more evenly arranged together, so that the molecules are not easy to be broken or wrinkled under high temperature and high pressure. The distance between them is longer, so that the plasticity, ductility and environmental stress cracking resistance are stronger, and it has better tensile properties and film durability, so that the film material can produce a stretching effect when heated during cooking, and is not easy to tear. HDPE is a highly crystalline, non-polar thermoplastic resin with high heat resistance and cold resistance, as well as high rigidity and toughness, good mechanical strength, good environmental stress cracking resistance, good high temperature resistance, and can maintain stability at a certain high temperature. It also has low permeability to water vapor and air, low water absorption, and high barrier properties. The cooking-resistant film made of specific amounts of each component has good mechanical properties, and after the heat-sealing layer contacts and heat-sealing layers, the modified heat-sealing material can improve the bonding tightness at the heat-sealing point, thereby increasing the heat-sealing strength and reducing the breakage rate during cooking.

[0009] Optionally, the modified heat sealing material comprises ULDPE, POP and EVA in a mass ratio of 1:0.7-1.1:0.8-1.2.

[0010] By adopting the above technical solution, ULDPE is an ultra-low density polyethylene with excellent flexibility and transparency. It is used as a compatibilizer for the modified heat-sealing material and the raw materials in the heat-sealing layer. Because it has certain similarities with HDPE and C6-LLDPE in molecular structure, it has good compatibility, so it can improve the compatibility of POP and EVA with the raw materials in the heat-sealing layer and increase the heat-sealing effect. Compared with PE, EVA (ethylene-vinyl acetate copolymer) introduces more vinyl acetate structural units in the macromolecular chain, has the characteristics of high impact resistance, outstanding flexibility and excellent heat sealing, and has a natural phase with the PE macromolecular chain structure. POP has good similarity with HDPE and ULDPE, so it has good compatibility with HDPE and ULDPE. POP is a polyolefin plastic with good barrier properties, which can effectively prevent the penetration of oxygen, water vapor and other gases, thereby improving the barrier properties of the cooking-resistant film and extending the shelf life of the packaging contents. In addition, POP also has good cream and chemical corrosion resistance, good stability, and improves transparency and flexibility to a certain extent. Therefore, using ULDPE, EVA and POP as modified heat-sealing materials can improve the heat-sealing strength between the heat-sealing layers to a certain extent, and after cooking, it still has good connection tightness and is not easy to burst or crack.

[0011] Optionally, plasma-modified ultra-high molecular weight polyethylene fibers are further added to the modified heat-sealing material, and the added amount of the plasma-modified ultra-high molecular weight polyethylene fibers is 2.5-3 wt % of the total amount of ULDPE, POP and EVA.

[0012] By adopting the above technical scheme, the ultra-high molecular weight polyethylene fiber has excellent mechanical properties and is called high-strength and high-modulus polyethylene fiber. However, since the interior is stacked with highly oriented methylene linear long chains, the molecular chain is composed of simple C and H elements, there is no active functional group, and the fiber surface is non-polar and smooth, the fiber surface free energy is low and the adhesion performance is poor, which limits the application of the ultra-high molecular weight polyethylene fiber. The ultra-high molecular weight polyethylene fiber is pretreated by a plasma treatment method to introduce functional groups such as carboxyl, carbonyl, and hydroxyl groups on its surface to improve its surface energy, thereby improving the compatibility of the ultra-high molecular weight polyethylene fiber with resins such as EVA. In the modified heat-sealing material, the tear resistance and tensile resistance of the cooking-resistant film can be increased, and it is not easy to burst during cooking. In addition, at the heat-sealed part, the stability of the heat-sealed connection can be increased, and the anti-cracking effect of the heat-sealed layer at high temperature can be increased.

[0013] Optionally, the preparation method of the plasma-modified ultra-high molecular weight polyethylene fiber is as follows: Add maleic acid to a polyvinyl alcohol solution with a concentration of 10-15wt%, stir evenly, add nano-hydrotalcite, and dry to obtain modified nano-hydrotalcite, wherein the mass ratio of maleic acid, hydrotalcite and polyvinyl alcohol is 1:0.15-0.2:0.1-0.2; The modified nano-hydrotalcite and the modified acrylic emulsion are uniformly mixed in a mass ratio of 0.6-0.8:1 to prepare a mixed solution; The ultra-high molecular weight polyethylene fiber is subjected to plasma treatment at 30-40 Pa for 3-7 minutes, immersed in the mixed solution for 3-5 minutes, and the ultra-high molecular weight polyethylene fiber is taken out and dried at 100-105°C.

[0014] By adopting the above technical scheme, nano hydrotalcite is a layered double metal hydroxide with exchangeable ions as anions between the layers, belonging to anionic clay. The nano sheet is evenly dispersed in the modified heat sealing material, which can greatly improve the barrier property of the film. Moreover, due to the special layered structure of nano hydrotalcite, it not only has a reinforcing effect, but also can improve the mechanical properties, thermal stability and barrier property. Polyvinyl alcohol is a synthetic polymer with a green and non-toxic processing process and biodegradability, but it has a large number of strongly polar hydroxyl groups and strong hydrophilicity. Therefore, food-grade non-toxic maleic acid is used as a cross-linking agent, and the hydroxyl groups in the polyvinyl alcohol molecules react with the carboxyl groups in the maleic acid molecules to undergo an esterification reaction, and ester carbonyl groups are introduced between the molecular chains, so that the binding force between the molecular chains becomes stronger and the free space density becomes smaller, so that the polyvinyl alcohol forms a dense coating on the surface of the hydrotalcite, and oxygen becomes difficult to penetrate between the polyvinyl alcohol chains, and the cross-linking agent is used to form a dense coating on the surface of the hydrotalcite. The cross-linking agent reduces the number of hydroxyl groups of polyvinyl alcohol, and the anions between the nano-hydrotalcite layers and the hydroxyl groups of polyvinyl alcohol can produce hydrogen bond interactions, which further reduces the hydroxyl content of polyvinyl alcohol, increases water resistance, and further improves the moisture barrier property of the nano-hydrotalcite. In the heat-sealing layer, the modified nano-hydrotalcite can provide a more tortuous diffusion path for gas molecules, thereby reducing the gas permeability. Since ester bonds appear between the cross-linked polyvinyl alcohol molecules, the hydroxyl groups on the repeating units react chemically with the carboxyl groups on the maleic acid molecules to form a three-dimensional network structure, thereby increasing the intermolecular force and the mechanical strength. In addition, the nano-hydrotalcite has good heat insulation ability, which can stop the thermal movement of the polymer chain in the mica during the cooking process, fix the polymer chain and free radicals, and prevent the diffusion of volatile decomposition products through the material. Therefore, it can be further added to increase the tear resistance and cooking resistance of the plastic film and improve the dimensional stability.

[0015] Plasma treatment increases the surface roughness of the ultra-high molecular weight polyethylene fiber and improves the contact area between the ultra-high molecular weight polyethylene fiber and the modified nano-hydrotalcite and the modified acrylic emulsion. The modified acrylic emulsion has adhesion and can load the modified nano-hydrotalcite on the ultra-high molecular weight polyethylene fiber treated with plasma through bonding. The modified acrylic emulsion has good waterproof and oil-proof effects, so it can further improve the barrier properties of the heat-sealing layer. Moreover, after forming a film on the ultra-high molecular weight polyethylene fiber, the coating is dense and uniform, and has good hydrophobicity, which can improve the dispersibility of the ultra-high molecular weight polyethylene fiber in materials such as EVA and POP, and can improve the heat-sealing strength and mechanical strength.

[0016] The modified nano-hydrotalcite can be dispersed more evenly in the modified acrylic emulsion due to the modification treatment. The adhesion effect of the modified acrylic emulsion is utilized to form evenly attached particles on the ultra-high molecular weight polyethylene fiber, thereby increasing the contact area between the ultra-high molecular weight polyethylene fiber and the raw materials in the heat-sealing layer during heat sealing, thereby improving the heat-sealing strength. During cooking, the ultra-high molecular weight polyethylene fiber can increase the tear resistance between the heat-sealing layers and prevent interlayer cracking.

[0017] Optionally, the density of POP in the modified heat-sealing material is 0.902 g / cm 3 , melt index is 1g / 10min, density of EVA is 0.94g / cm 3 , melt index is 5.5g / 10min, density of ULDPE is 0.905g / cm 3 , the melt index is 0.8g / 10min.

[0018] Optionally, the density of HDPE in the corona layer is 0.9561 g / cm 3 , the melt index is 7.34g / 10min, and the density of C6-LLDPE is 0.92g / cm 3 , melt index is 1g / 10min; The density of HDPE in the middle layer is 0.9561 g / cm 3 , the melt index is 7.34g / 10min, and the density of C6-LLDPE is 0.92g / cm 3 , the melt index is 1g / 10min, the density of C4-LLDPE is 0.918g / cm3, the melt index is 2g / 10min; the density of HDPE in the heat seal layer is 0.9561g / cm 3 , the melt index is 7.34g / 10min, and the density of C6-LLDPE is 0.92g / cm 3 , the melt index is 1g / 10min.

[0019] Optionally, the thickness ratio of the corona layer, the intermediate layer and the heat-sealing layer is 4.5-5:2.5-3:2.5.

[0020] By adopting the above technical scheme, the thickness of each layer of the retort-resistant film is reasonably adjusted, so that the retort-resistant film has better heat sealing strength and tear resistance, and the film layer of this structure has better tensile resistance and retort-resistant effect.

[0021] Optionally, the processing aid is selected from at least one of a plasticizer, a compatibilizer, an antioxidant, a cross-linking agent and an opening lubricant.

[0022] In the second aspect, the present application provides a method for preparing a cast CPE cooking-resistant film, adopting the following technical scheme: a method for preparing a cast CPE cooking-resistant film, comprising the following steps: respectively mixing the raw materials in the corona layer, the intermediate layer and the heat sealing layer evenly, melting, and cast extruding, and then passing through a cooling roller at 34-38°C, coronaing to a dyne value of 40, winding, aging, and slitting.

[0023] By adopting the above technical scheme, the raw materials of each layer are mixed evenly, added into the extruder for cast extrusion, cooled by the cooling roller to form a film, and then corona treatment is performed. The aging rack can make the processing aids in the film enter and migrate effectively.

[0024] In summary, this application has the following beneficial effects: 1. Since the present application adopts a special amount of HDPE and C6-LLDPE, C4-LLDPE and modified heat sealing materials and processing aids for reasonable allocation, the raw material dosage of the corona layer, the middle layer and the heat sealing layer is obtained to make a cooking-resistant film with good tensile strength, impact strength and heat sealing strength, which is not easy to produce interlayer peeling after cooking.

[0025] 2. In the present application, POP, ULDPE and EVA are preferably used as modified heat sealing materials, and a certain amount of plasma-modified ultra-high molecular weight polyethylene fiber is added, so that the modified heat sealing material can further increase the connection strength of the heat seal and further improve the tensile and tear strength of the plastic film.

[0026] 3. In the present application, it is preferred to use modified nano-hydrotalcite, modified acrylic emulsion, etc. to treat the ultra-high molecular weight polyethylene fiber to obtain a fiber with increased surface roughness and hydrophobicity, and a certain amount of modified nano-hydrotalcite is attached to increase the connection strength between the heat-sealing layer and the heat-sealing layer at the heat-sealing portion, and increase the barrier capacity of the plastic film. DETAILED DESCRIPTION

[0027] The following examples further illustrate the present application in detail.

[0028] Preparation Example 1-13 of Modified Heat Sealing Material Preparation Example 1: 100g ULDPE, 100g POP and 100g EVA were mixed evenly and extruded and granulated at 180°C to obtain a modified heat-sealing material. The density of POP was 0.902g / cm 3 , melt index is 1g / 10min, selected from Dow Chemical, USA, brand is 1880G, EVA density is 0.94g / cm 3 , melt index is 5.5g / 10min, selected from DuPont, USA, brand 53009, ULDPE density is 0.905g / cm 3 The melt index is 0.8g / 10min, selected from Dow Chemical of the United States, model 4203.

[0029] Preparation Example 2: 100g ULDPE, 110g POP and 120g EVA were mixed evenly and extruded and granulated at 180°C to obtain a modified heat-sealing material. The density of POP was 0.902g / cm 3 , melt index is 1g / 10min, selected from Dow Chemical, USA, brand is 1880G, EVA density is 0.94g / cm 3 , melt index is 5.5g / 10min, selected from DuPont, USA, brand 53009, ULDPE density is 0.905g / cm 3 The melt index is 0.8g / 10min, selected from Dow Chemical of the United States, model 4203.

[0030] Preparation Example 3: 100g ULDPE, 70g POP and 80g EVA were mixed evenly and extruded and granulated at 180°C to obtain a modified heat-sealing material. The density of POP was 0.902g / cm 3 , melt index is 1g / 10min, selected from Dow Chemical, USA, brand is 1880G, EVA density is 0.94g / cm 3 , melt index is 5.5g / 10min, selected from DuPont, USA, brand 53009, ULDPE density is 0.905g / cm 3 The melt index is 0.8g / 10min, selected from Dow Chemical of the United States, model 4203.

[0031] Preparation Example 4: The difference from Preparation Example 1 is that an equal amount of POP is used to replace ULDPE.

[0032] Preparation Example 5: The difference from Preparation Example 1 is that an equal amount of POP is used instead of EVA.

[0033] Preparation Example 6: The difference from Preparation Example 1 is that no POP is added.

[0034] Preparation Example 7: 100g ULDPE, 100g POP and 100g EVA are mixed evenly, and 3wt% of the total weight of the three is added into plasma-modified ultra-high molecular weight polyethylene fiber. The preparation method of plasma-modified ultra-high molecular weight polyethylene fiber is as follows: after the ultra-high molecular weight polyethylene fiber is evenly dispersed, it is plasma treated for 3 minutes at a pressure of 40Pa. The ultra-high molecular weight polyethylene fiber is selected from Shandong Luxian Building Materials Technology Co., Ltd., with a length of 12mm, a diameter of 5μm, and a model of LXPE.

[0035] Preparation Example 8: 100g ULDPE, 100g POP and 100g EVA are mixed evenly, and 2.5wt% of the total weight of the three plasma-modified ultra-high molecular weight polyethylene fibers are added. The preparation method of the plasma-modified ultra-high molecular weight polyethylene fibers is as follows: the ultra-high molecular weight polyethylene fibers are evenly dispersed and then plasma treated for 3 minutes at a pressure of 40Pa. The ultra-high molecular weight polyethylene fibers are selected from Shandong Luxian Building Materials Technology Co., Ltd., with a length of 12mm, a diameter of 5μm, and a model of LXPE.

[0036] Preparation Example 9: The difference from Preparation Example 7 is that the plasma-modified ultra-high molecular weight polyethylene fiber is prepared by the following method: (1) 150 g of polyvinyl alcohol 1788 and 850 g of deionized water were mixed and stirred to dissolve in an oil bath at 85° C. to prepare a polyvinyl alcohol solution with a concentration of 15 wt %; (2) maleic acid was added to a 15 wt % polyvinyl alcohol solution, and after stirring, nano-hydrotalcite was added, and the mixture was stirred at 95 ° C for 4 h, and dried at 80 ° C for 10 h to obtain modified nano-hydrotalcite, wherein the mass ratio of maleic acid, hydrotalcite and polyvinyl alcohol was 1:0.2:0.2, polyvinyl alcohol was selected from Shandong Tengxiao New Materials Co., Ltd., with a product number of 088-20, maleic acid was selected from Shandong Baiqianhui Biotechnology Co., Ltd., with a product number of 56, and nano-hydrotalcite was selected from Shanghai Wanzhao Fine Chemical Co., Ltd., with a model of WSG, a product number of 432, and a particle size of 300 mesh; (3) mixing the modified nano-hydrotalcite and the modified acrylic emulsion in a mass ratio of 0.8:1 to obtain a mixed solution, wherein the modified acrylic emulsion is selected from Foshan Zhaojing Environmental Protection Technology Co., Ltd., and the product number is AU6183; (4) The ultra-high molecular weight polyethylene fiber was plasma treated at 40 Pa for 3 minutes, immersed in the mixed solution for 5 minutes, and the ultra-high molecular weight polyethylene fiber was taken out and dried at 100°C. The ultra-high molecular weight polyethylene fiber was selected from Shandong Luxian Building Materials Technology Co., Ltd., with a length of 12 mm, a diameter of 5 μm, and a model of LXPE.

[0037] Preparation Example 10: The difference from Preparation Example 7 is that the plasma-modified ultra-high molecular weight polyethylene fiber is prepared by the following method: (1) 100 g of polyvinyl alcohol 1788 and 900 g of deionized water were mixed and stirred in an oil bath at 85° C. to dissolve to prepare a polyvinyl alcohol solution with a concentration of 10 wt %; (2) maleic acid was added to a 10 wt % polyvinyl alcohol solution, and after stirring, nano-hydrotalcite was added, and the mixture was stirred at 95 ° C for 4 h, and dried at 80 ° C for 10 h to obtain modified nano-hydrotalcite, wherein the mass ratio of maleic acid, hydrotalcite and polyvinyl alcohol was 1:0.15:0.1, polyvinyl alcohol was selected from Shandong Tengxiao New Materials Co., Ltd., with a product number of 088-20, maleic acid was selected from Shandong Baiqianhui Biotechnology Co., Ltd., with a product number of 56, and nano-hydrotalcite was selected from Shanghai Wanzhao Fine Chemical Co., Ltd., with a model of WSG, a product number of 432, and a particle size of 300 mesh; (3) mixing the modified nano-hydrotalcite and the modified acrylic emulsion in a mass ratio of 0.6:1 to obtain a mixed solution, wherein the modified acrylic emulsion is selected from Foshan Zhaojing Environmental Protection Technology Co., Ltd., and the product number is AU6183; (4) The ultra-high molecular weight polyethylene fiber was plasma treated at 40 Pa for 3 minutes, immersed in the mixed solution for 3 minutes, and the ultra-high molecular weight polyethylene fiber was taken out and dried at 105°C. The ultra-high molecular weight polyethylene fiber was selected from Shandong Luxian Building Materials Technology Co., Ltd., with a length of 12 mm, a diameter of 5 μm, and a model of LXPE.

[0038] Preparation Example 11: The difference from Preparation Example 9 is that the nano-hydrotalcite is not modified by polyvinyl alcohol and maleic acid, and the nano-hydrotalcite is mixed with modified acrylic ester emulsion in a mass ratio of 0.8:1 to prepare a mixed solution.

[0039] Preparation Example 12: The difference from Preparation Example 9 is that an equal amount of a 20% carrageenan aqueous solution is used to replace the modified acrylic ester emulsion.

[0040] Preparation Example 13: The difference from Preparation Example 9 is that no modified nano-hydrotalcite is added to the mixed liquid, and only modified acrylic ester emulsion is used as the mixed liquid. Example

[0041] Example 1: A cast CPE cooking-resistant film with a thickness of 0.08 mm, comprising a corona layer, an intermediate layer and a heat-sealing layer in contact with each other in sequence, wherein the thickness ratio of the corona layer, the intermediate layer and the heat-sealing layer is 5:2.5:2.5, and the amount of raw materials used in each layer (kg) is shown in Table 1. The density of HDPE in the corona layer is 0.9561 g / cm 3 , the melt index is 7.34g / 10min, and the density of C6-LLDPE is 0.92g / cm 3The melt index is 1g / 10min, and the added additives include an antioxidant and an opening lubricant with a mass ratio of 1:1. The antioxidant is 1010, and the opening lubricant is oleic acid amide; the density of HDPE in the middle layer is 0.9561g / cm 3 , the melt index is 7.34g / 10min, and the density of C6-LLDPE is 0.92g / cm 3 , melt index is 1g / 10min, density of C4-LLDPE is 0.918g / cm 3 , the melt index is 2g / 10min; the density of HDPE in the heat seal layer is 0.9561g / cm 3 , the melt index is 7.34g / 10min, and the density of C6-LLDPE is 0.92g / cm 3 , the melt index is 1g / 10min, the processing aid is a plasticizer and a compatibilizer in a mass ratio of 1:1, the plasticizer is propylene glycol, the compatibilizer is acrylic acid, and the heat-sealing modified material is prepared by Preparation Example 1.

[0042] The method for preparing the cast CPE boiling-resistant film comprises the following steps: S1. According to the amount in Table 1, the raw materials used for the corona layer, the middle layer and the heat-sealing layer were weighed, respectively poured into a stirrer, stirred for 20 min, added into an extruder after stirring, and cast extruded. The temperature settings of the corona layer in the extruder were: 180 ° C in one zone, 200 ° C in two zones, 220 ° C in three zones, 225 ° C in four zones, and 230 ° C in five zones. The temperature settings of the middle layer in each zone were: 180 ° C in one zone, 200 ° C in two zones, 220 ° C in three zones, 230 ° C in four zones, and 245 ° C in five zones; the temperature settings of the heat-sealing layer in each zone were: 180 ° C in one zone, 22 ° C in two zones, 240 ° C in three zones, 250 ° C in four zones, and 250 ° C in five zones; 225 ° C in one zone of the die, 225 ° C in two zones, 225 ° C in three zones, 225 ° C in four zones, and 225 ° C in five zones; S2, passing each layer of the cast extruded film through a cooling roller with a water temperature of 36°C and a vacuum machine speed of 1350r / min; S3, the thickness of the thickness gauge is set at 80MIC (0.08mm), the standard deviation is set at 3%, and the automatic die head online PID is turned on to adjust the film thickness; S4, using a corona machine to perform corona treatment on the corona layer, and the corona value reaches 40 dynes; S5, rolling up the corona-treated composite film online, with the number of meters of each roll being 8000 meters; S6. The semi-finished products after unwinding are placed on the aging rack for 48 hours of aging, and then cut into standard widths and packaged for storage.

[0043] Table 1 Raw material dosage of cast CPE cooking-resistant film in Examples 1-3 Example 2: A cast CPE cooking-resistant film, which is different from Example 1 in that the amounts of raw materials are as shown in Table 1, and the heat-sealing modified material in the heat-sealing layer is made from Preparation Example 2.

[0044] Example 3: A cast CPE cooking-resistant film, which is different from Example 1 in that the amounts of raw materials are as shown in Table 1, and the heat-sealing modified material in the heat-sealing layer is made from Preparation Example 3.

[0045] Example 4: A cast CPE cooking-resistant film, which is different from Example 1 in that the thickness ratio of the corona layer, the middle layer and the heat-sealing layer is 4.5:3:2.5.

[0046] Example 5: A cast CPE cooking-resistant film, which is different from Example 1 in that the thickness ratio of the corona layer, the middle layer and the heat-sealing layer is 5:3:2.5.

[0047] Example 6: A cast CPE cooking-resistant film, which is different from Example 1 in that the heat-seal modified material in the heat-seal layer is made from Preparation Example 4.

[0048] Example 7: A cast CPE cooking-resistant film, which is different from Example 1 in that the heat-sealing modified material in the heat-sealing layer is made from Preparation Example 5.

[0049] Example 8: A cast CPE cooking-resistant film, which is different from Example 1 in that the heat-sealing modified material in the heat-sealing layer is made from Preparation Example 6.

[0050] Example 9: A cast CPE cooking-resistant film, which is different from Example 1 in that the heat-seal modified material in the heat-seal layer is made from Preparation Example 7.

[0051] Example 10: A cast CPE cooking-resistant film, which is different from Example 1 in that the heat-seal modified material in the heat-seal layer is made from Preparation Example 8.

[0052] Example 11: A cast CPE cooking-resistant film, which is different from Example 9 in that the heat-seal modified material in the heat-seal layer is made from Preparation Example 9.

[0053] Example 12: A cast CPE cooking-resistant film, which is different from Example 9 in that the heat-seal modified material in the heat-seal layer is made from Preparation Example 10.

[0054] Example 13: A cast CPE cooking-resistant film, which is different from Example 11 in that the heat-seal modified material in the heat-seal layer is made from Preparation Example 11.

[0055] Example 14: A cast CPE cooking-resistant film, which is different from Example 11 in that the heat-seal modified material in the heat-seal layer is made from Preparation Example 12.

[0056] Example 15: A cast CPE cooking-resistant film, which is different from Example 11 in that the heat-seal modified material in the heat-seal layer is made from Preparation Example 13.

[0057] Comparative Example Comparative Example 1: A cast CPE cooking-resistant film, which differs from Example 1 in that an equal amount of mLLDPE is used to replace the modified heat-sealing material in the heat-sealing layer, and the melt index of mLLDPE is 0.5 g / 10 min and the density is 0.92 g / cm 3 , selected from Dow 5520G, USA.

[0058] Comparative Example 2: A cast CPE cooking-resistant film, which differs from Example 1 in that C4-LLDPE is used in an equal amount to replace C6-LLDPE in the heat sealing layer, the density of C4-LLDPE is 0.918 g / cm3, the melt index is 2 g / 10min, and the model is 1002BU.

[0059] Comparative Example 3: A method for preparing a polyethylene film, comprising the following steps: Composite layer resin raw materials, intermediate layer resin raw materials and heat sealing layer resin raw materials are respectively added into the three barrels of the co-extrusion machine, and the formulas of each resin raw material are as follows: composite layer: 32wt% LDPE, 32wt% LLDPE and 36wt% modified m-LLDPE; intermediate layer: 30wt% LDPE, 60wt% LLDPE and 10wt% white masterbatch; heat sealing layer: 31wt% LDPE and 69wt% LLDPE, LDPE are TN00 provided by China Petroleum & Chemical Corporation, LLDPE are 1002YB provided by Exxon Corporation, modified m-LLDPE are 5401 provided by Dow Chemical Company, white masterbatch are UF880 provided by DIC Corporation, and adhesives are UK3640 provided by Henkel AG of Germany.

[0060] The polymer particles in the above three barrels are melted by the extruder to form a tube billet. After the tube billet is stretched, compressed air is rushed out from the center of the extruder die to blow the tube billet into a bubble film. At the same time, the bubble film is cooled and shaped by air ring cooling wind to obtain a PE film. The composite layer zone 1 is 130℃, zone 2 is 140℃, zone 3 is 150℃, zone 4 is 150℃, the middle layer zone 1 is 120℃, zone 2 is 130℃, zone 3 is 150℃, zone 4 is 150℃, the heat sealing layer zone 1 is 130℃, zone 2 is 140℃, zone 3 is 150℃, zone 4 is 150℃, and the die is 150℃.

[0061] Performance testing Plastic films were prepared according to the methods in the examples and comparative examples, and performance tests were performed according to the following methods. The test results are recorded in Table 2.

[0062] 1. Tensile strength: Test according to GB / T13022-1991 "Test method for tensile properties of plastic films".

[0063] 2. Elongation at break: Tested in accordance with GB / T13022-1991 “Test method for tensile properties of plastic films”.

[0064] 3. Tear force: Tested in accordance with GB / T16578.1-2008 “Determination of tear resistance of plastic film and sheeting Part 1: Trouser tear method”.

[0065] 4. Heat seal strength: Heat seal the heat seal layer and the corona layer, and the heat seal layer and the heat seal layer at 125°C, and test according to QB / T2358-1998 "Test method for heat seal strength of plastic film packaging bags", and then cook at 121°C for 30 minutes and measure the heat seal strength of the heat seal again.

[0066] 5. Water vapor permeability: Tested in accordance with GB / T1038-2022 "Test method for gas permeability of plastic films and sheets - Part 1: Differential pressure method".

[0067] 6. Oxygen permeability: Test in accordance with GB / T19789-2005 “Oxygen permeability test for plastic films and sheets for packaging materials - Coulometer test method”.

[0068] Table 2 It can be seen from the data in Table 2 that Examples 1-3 respectively use the heat-seal modified materials prepared in Preparation Examples 1-3, and the prepared cooking-resistant films have high heat-seal strength and tight adhesion. After high-temperature cooking at 121°C, the films have strong heat-seal effect and good stress cracking resistance. The heat-seal mouth is not easy to break, and the surface does not deform or wrinkle, and there is no delamination and separation between layers.

[0069] In Example 4 and Example 5, the thickness ratios among the corona layer, the intermediate layer and the heat-sealing layer are adjusted, and the cooking-resistant films thus prepared have mechanical properties such as tensile strength similar to those of Example 1.

[0070] In Example 6, Example 7 and Example 8, the modified heat-sealing materials prepared in Preparation Example 4, Preparation Example 5 and Preparation Example 6 were used respectively. The data in Table 2 show that the retort-resistant films prepared in Examples 6-8 have decreased mechanical properties such as tensile strength and tear force, and the heat-sealing properties are affected to a certain extent, and the barrier properties are slightly decreased.

[0071] In Example 9 and Example 10, the modified heat sealing materials prepared in Preparation Example 7 and Preparation Example 8 are used respectively, and a certain amount of plasma-modified ultra-high molecular weight polyethylene fiber is further added to the modified heat sealing material. The data in Table 2 show that the tensile resistance and tear resistance of the retort bags prepared in Example 9 and Example 10 are improved, and the heat sealing strength is further improved. The heat sealing strength is still high after retort, and the heat seal is not easy to burst or crack.

[0072] In Example 11 and Example 12, the modified heat sealing materials prepared in Preparation Example 9 and Preparation Example 10 are respectively used, wherein the plasma-treated ultra-high molecular weight polyethylene fiber is treated with modified nano-hydrotalcite and modified acrylic emulsion. Compared with Example 9, the cooking-resistant film prepared thereby not only has increased heat sealing strength, and the heat sealing strength at the heat seal is stable, but also the cooking-resistant film has improved barrier properties against water vapor and oxygen.

[0073] Compared with Example 11, the modified heat sealing material prepared in Preparation Example 11 is used, in which polyvinyl alcohol and maleic acid are not used to modify the nano-hydrotalcite. It can be seen that the water vapor permeability of the cooking-resistant film is increased, and the heat sealing strength is reduced. It may be that it is difficult to disperse the nano-hydrotalcite evenly in the modified acrylic ester emulsion, which makes it unevenly distributed on the ultra-high molecular weight polyethylene fiber, resulting in difficulty in heat sealing tightly.

[0074] Compared with Example 11, Example 14 uses the modified heat sealing material prepared in Preparation Example 12, wherein a carrageenan aqueous solution is used instead of the modified acrylic emulsion. Compared with the effect in Example 11, the barrier properties of the boiling-resistant film are reduced and the boiling-resistant effect is weakened.

[0075] In Example 15, the modified heat sealing material prepared in Preparation Example 13 was used. Compared with Example 11, the data in Table 2 showed that the mechanical properties of the cooking-resistant film prepared in Example 15 were improved, but the improvement effect on the barrier properties was not good.

[0076] In Comparative Example 1, mLLDPE is used in equal amount to replace the modified heat-sealing material. It can be seen that the heat-sealing strength of the film material prepared in Comparative Example 1 decreases, and after steaming, the heat-sealing strength decreases significantly.

[0077] Compared with Example 1, Comparative Example 2 uses C4-LLDPE instead of C6-LLDPE in the heat sealing layer. Table 2 shows that the mechanical strength of the cooking-resistant film prepared in Comparative Example 2 decreases and the heat sealing performance becomes worse.

[0078] Comparative Example 3 is a plastic film prepared by the prior art, which has poor tensile strength and tear resistance, and after being steamed, the heat sealing strength at the heat sealing portion decreases, and cracking is easily generated.

[0079] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A cast CPE boiling-resistant film, characterized in that: It comprises a corona layer, an intermediate layer and a heat-sealing layer which are in contact with each other in sequence, wherein the corona layer comprises the following raw materials in weight percentage: 55-60% HDPE, 37-42% C6-LLDPE, and the balance is a processing aid; The middle layer comprises the following raw materials in weight percentage: HDPE 60-65%, C6-LLDPE 27-30%, C4-LLDPE 8-10%; The heat sealing layer comprises the following raw materials in weight percentage: 50-55% HDPE, 25-30% C6-LLDPE, 13-15% modified heat sealing material, and the balance is processing aid.

2. The cast CPE boiling-resistant film according to claim 1, characterized in that: The modified heat-sealing material comprises ULDPE, POP and EVA in a mass ratio of 1:0.7-1.1:0.8-1.

2.

3. The cast CPE boiling-resistant film according to claim 2, characterized in that: The modified heat-sealing material is further added with plasma-modified ultra-high molecular weight polyethylene fiber, and the added amount of the plasma-modified ultra-high molecular weight polyethylene fiber is 2.5-3wt% of the total amount of ULDPE, POP and EVA.

4. The cast CPE boiling-resistant film according to claim 3, characterized in that: The preparation method of the plasma-modified ultra-high molecular weight polyethylene fiber is as follows: Add maleic acid to a polyvinyl alcohol solution with a concentration of 10-15wt%, stir evenly, add nano-hydrotalcite, and dry to obtain modified nano-hydrotalcite, wherein the mass ratio of maleic acid, hydrotalcite and polyvinyl alcohol is 1:0.15-0.2:0.1-0.2; The modified nano-hydrotalcite and the modified acrylic emulsion are uniformly mixed in a mass ratio of 0.6-0.8:1 to prepare a mixed solution; The ultra-high molecular weight polyethylene fiber is subjected to plasma treatment at 30-40 Pa for 3-7 minutes, immersed in the mixed solution for 3-5 minutes, and the ultra-high molecular weight polyethylene fiber is taken out and dried at 100-105°C.

5. The cast CPE boiling-resistant film according to claim 2, characterized in that: The density of POP in the modified heat sealing material is 0.902 g / cm 3 , melt index is 1g / 10min, density of EVA is 0.94g / cm 3 , melt index is 5.5g / 10min, density of ULDPE is 0.905g / cm 3 , the melt index is 0.8g / 10min.

6. The cast CPE boiling-resistant film according to claim 5, characterized in that: The density of HDPE in the corona layer is 0.9561 g / cm 3 , the melt index is 7.34g / 10min, and the density of C6-LLDPE is 0.92g / cm 3 , melt index is 1g / 10min; The density of HDPE in the middle layer is 0.9561 g / cm 3 , the melt index is 7.34g / 10min, and the density of C6-LLDPE is 0.92g / cm 3 , melt index is 1g / 10min, density of C4-LLDPE is 0.918g / cm3, melt index is 2g / 10min; The density of HDPE in the heat seal layer is 0.9561 g / cm 3 , the melt index is 7.34g / 10min, and the density of C6-LLDPE is 0.92g / cm 3 , the melt index is 1g / 10min.

7. The cast CPE boiling-resistant film according to claim 1, characterized in that: The thickness ratio of the corona layer, the middle layer and the heat-sealing layer is 4.5-5:2.5-3:2.

5.

8. The cast CPE boiling-resistant film according to claim 1, characterized in that: The processing aid in the corona layer and the heat-sealing layer is selected from at least one of a plasticizer, a compatibilizer, an antioxidant, a cross-linking agent and an opening lubricant.

9. The method for preparing the cast CPE boiling-resistant film according to any one of claims 1 to 8, characterized in that: The following steps are involved: The raw materials in the corona layer, the middle layer and the heat-sealing layer are respectively mixed evenly, melted, cast and extruded, and then passed through a cooling roller at 34-38°C, coronaed to 40 dyne value, and then rolled, aged and slit.

Citation Information

Patent Citations

  • CPE heat-sealing composite film and preparation method thereof

    CN110466225A

  • Easily-uncovered film for high-temperature cooking sealing cover and preparation method of easily-uncovered film

    CN116787893A

Cited By

  • Nine-layer upward-blowing asymmetric PE / PA soft packaging film and preparation method thereof

    CN119704831A