High-strength PE film, preparation method thereof and packaging bag

Through the three-layer coextrusion and blowing film technology, a high-strength PE film is prepared using a specific proportion of MLLDPE, EVA, LDPE and PPA materials, which solves the problem of insufficient compression and drop resistance in transportation of the packaging bag, achieving good results physical performance and production efficiency.

CN119017805APending Publication Date: 2024-11-26珠海市德燊环保包装有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411040298.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing packaging bags are prone to bumps and falls during transportation, lack good compressive strength and drop resistance, making it difficult to meet the needs of plastic reduction and cost reduction.

Method used

Using three-layer coextrusion blown film technology, the inner layer, middle layer and outer layer consist of specific proportions of MLLDPE, EVA, LDPE and PPA. By adjusting the formulation and process parameters, such as temperature and blowing ratio, a high tensile strength is prepared. , PE film with good heat sealing performance, drop resistance and compressive strength.

Benefits of technology

The PE film has achieved a comprehensive improvement of good tensile strength, heat sealing performance, drop resistance and compressive strength, which meets the impact resistance of packaging bags in transportation and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention provides a high-strength PE film which comprises a three-layer co-extrusion layer formed by three-layer co-extrusion film blowing, the three-layer co-extrusion layer comprises an inner layer, a middle layer and an outer layer, the inner layer comprises MLLDPE, EVA, LLDPE and PPA, the middle layer comprises MLLDPE, LDPE, LLDPE and PPA, and the outer layer comprises MLLDPE, LDPE, LLDPE and PPA. The invention further provides a preparation method of the PE film and a packaging bag prepared from the PE film. The PE film provided by the invention has good tensile strength and good heat sealability, and also has good drop resistance and high compressive strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of PE film, specifically to a high-strength PE film, its preparation method, and packaging bags. Background Technology

[0002] Driven by the need to reduce plastic use and lower costs, an increasing number of daily chemical products are switching from bottle and can packaging to stand-up pouches or spout pouches. During transportation, these pouches inevitably experience bumps and knocks, and may even fall from heights. Therefore, developing packaging film with good compressive strength and impact resistance is essential. Summary of the Invention

[0003] In order to overcome the shortcomings of the prior art, the purpose of this invention is to provide a PE film with good tensile strength and good heat-sealing performance, as well as good impact resistance and high compressive strength.

[0004] To solve the above problems, the technical solution adopted by the present invention is as follows:

[0005] A high-strength PE film includes a three-layer co-extruded layer formed by three-layer co-extrusion blown film. The three-layer co-extruded layer includes an inner layer, a middle layer and an outer layer. The inner layer includes MLLDPE, EVA, LLDPE and PPA. The middle layer includes MLLDPE, LDPE, LLDPE and PPA. The outer layer includes MLLDPE, LDPE, LLDPE and PPA.

[0006] In some possible implementations, the components of the inner layer are as follows by weight percentage:

[0007]

[0008]

[0009] The components of the middle layer are as follows by weight percentage:

[0010]

[0011] The components of the outer layer are as follows by weight percentage:

[0012]

[0013] In some possible implementations, the MLLDPE is model number 1018MF, the EVA is model number 3172Z, the LDPE is model number 2426K, the PPA is model number A1058, the LLDPE in the inner layer is model number 1002BU, and the LLDPE in the middle and outer layers is model number 7042.

[0014] In some possible implementations, the middle layer component further includes 3%–5% white masterbatch, which is of type LE8236, by weight percentage.

[0015] In some possible implementations, the thickness of the inner layer is 33% of the total thickness of the film, the thickness of the middle layer is 33% of the total thickness of the film, and the thickness of the outer layer is 34% of the total thickness of the film.

[0016] This application also provides a method for preparing a high-strength PE film, wherein the preparation method uses the components of each layer of the high-strength PE film, and the preparation method includes the following steps:

[0017] After the components of the inner layer are mixed evenly, they are fed into the inner layer hopper of the three-layer co-extrusion blown film machine;

[0018] After the components of the middle layer are mixed evenly, they are fed into the middle layer hopper of the three-layer co-extrusion blown film machine;

[0019] After the components of the outer layer are mixed evenly, they are fed into the outer hopper of the three-layer co-extrusion blown film machine.

[0020] The three-layer co-extrusion blown film machine melts and extrudes the components in each hopper through each extrusion screw to the die head to blow into the PE film.

[0021] In some possible implementations, the inner screw barrel temperature is 175-185°C, the middle screw barrel temperature is 185-195°C, the outer screw barrel temperature is 175-180°C, the flow channel temperature of the die head is 185-190°C, and the die opening temperature is 185°C.

[0022] In some possible implementations, the inflation ratio is 2.5–3.0.

[0023] In some possible implementations, the air-cooling temperature is 15-18°C, and the operating frequency of the cooling fan is greater than or equal to 45Hz.

[0024] This application also provides a packaging bag made using the aforementioned high-strength PE film.

[0025] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0026] In this application, by adjusting the PE formulation, the composite PE film has good tensile strength and good heat-sealing performance, as well as good drop resistance and high compressive strength.

[0027] The present invention will be further described in detail below with reference to specific embodiments. Detailed Implementation

[0028] The technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.

[0030] The following describes some embodiments of the present invention in detail. Unless otherwise specified, the following embodiments and features can be combined with each other.

[0031] One embodiment of this application provides a high-strength PE film, comprising a three-layer co-extruded layer formed by three-layer co-extrusion blown film. The three-layer co-extruded layer includes an inner layer, a middle layer, and an outer layer. The inner layer includes MLLDPE, EVA, LLDPE, and PPA. The middle layer includes MLLDPE, LDPE, LLDPE, and PPA. The outer layer includes MLLDPE, LDPE, LLDPE, and PPA.

[0032] MLLDPE is short for metallocene linear low-density polyethylene, EVA is short for ethylene-vinyl acetate copolymer, LLDPE is linear low-density polyethylene, and PPA is a processing aid. It is a mixture, with the commercial name code DS-A1058, and is a product of Beijing Yalen Zhilian Technology Co., Ltd. LDPE is short for low-density polyethylene. In this embodiment, the addition of PPA has the following advantages: improved surface gloss and smoothness of the plastic film; elimination of sharkskin and watermarks caused by melt fracture; reduction of crystal points caused by equipment and raw material factors; reduction of extruder current and pressure under unchanged equipment and process conditions, thereby improving equipment production efficiency; reduction of die temperature, improved film bubble stability, improved plasticizing function of basic equipment, improved melt flowability, and improved overall product performance.

[0033] In some embodiments, the components of the inner layer are as follows by weight percentage:

[0034]

[0035] The components of the middle layer are as follows by weight percentage:

[0036]

[0037] The components of the outer layer are as follows by weight percentage:

[0038]

[0039] In some embodiments, the MLLDPE is of type 1018MF, which is beneficial for further increasing thermal adhesion and puncture resistance; the EVA is of type 3172Z, which is beneficial for further increasing thermal adhesion and low-temperature heat-sealing properties; the LDPE is of type 2426K, which has a stabilizing effect on the film bubble, thereby helping to ensure the overall quality of the PE film; the PPA is of type A1058; in the inner layer, the LLDPE is of type 1002BU; and in the middle and outer layers, the LLDPE is of type 7042. LLDPE of type 1002BU is beneficial for further increasing the tensile strength and toughness of the film.

[0040] In some embodiments, the middle layer component further comprises 3%-5% white masterbatch by weight, wherein the white masterbatch is of type LE8236 (manufactured by Guangdong Yilong New Material Technology Co., Ltd.). The masterbatch of the above proportion has good compatibility with the functional components of this application, thereby facilitating a better coloring effect on the film.

[0041] In some embodiments, the thickness of the inner layer is 33% of the total thickness of the film, the thickness of the middle layer is 33% of the total thickness of the film, and the thickness of the outer layer is 34% of the total thickness of the film. These thickness settings allow for better coloring results with less masterbatch.

[0042] Another embodiment of this application provides a method for preparing a high-strength PE film, wherein the preparation method uses the components of each layer of the high-strength PE film described in the above embodiments, and the preparation method includes the following steps:

[0043] After the components of the inner layer are mixed evenly, they are fed into the inner layer hopper of the three-layer co-extrusion blown film machine.

[0044] After the components of the middle layer are mixed evenly, they are fed into the middle layer hopper of the three-layer co-extrusion blown film machine.

[0045] After the components of the outer layer are mixed evenly, they are fed into the outer hopper of the three-layer co-extrusion blown film machine.

[0046] The feeding sequence of the above-mentioned hoppers can be changed or is not important.

[0047] The three-layer co-extrusion blown film machine melts and extrudes the components in each hopper through each extrusion screw to the die head to blow into the PE film.

[0048] In some embodiments, the inner screw barrel temperature is 175-185°C, the middle screw barrel temperature is 185-195°C, the outer screw barrel temperature is 175-180°C, the die runner temperature is 185-190°C, and the die opening temperature is 185°C. The selection of these temperatures has the following advantages: 1. Ensures good material plasticization: Suitable temperatures allow polyethylene to fully melt and plasticize, ensuring material flowability and uniformity, thereby achieving good extrusion quality. 2. Optimizes product performance: Different temperature settings help adjust the molecular structure and crystallinity of each layer of material, thereby improving the physical properties of the product, such as strength, toughness, and transparency. 3. Improves production efficiency: Appropriate temperatures can reduce the residence time of material in the barrel, reducing the risk of material decomposition and degradation, improving the continuity and stability of production, and thus increasing production efficiency. 4. Reduces energy consumption: Reasonable temperature control can avoid energy waste caused by overheating and reduce production costs.

[0049] In some embodiments, the blow-up ratio is 2.5–3.0. The advantages of this blow-up ratio include: controlling film thickness uniformity: a suitable blow-up ratio helps to make the film thickness distribution more uniform in the transverse direction, reducing thickness deviations and thus improving the consistency of product quality and performance. Optimizing film physical properties: it helps to adjust the tensile strength, toughness, transparency, and other physical properties of the film to meet the needs of different application scenarios. For example, appropriately increasing the blow-up ratio can improve the transverse tensile strength and toughness of the film. Improving film optical properties: it can affect the transparency and gloss of the film; a suitable blow-up ratio can give the film better optical properties, resulting in better appearance in packaging and other fields. Improving production efficiency and stability: it helps to stabilize the production process, reduce scrap and production interruptions caused by problems such as uneven thickness and unstable performance, thereby improving production efficiency and reducing costs.

[0050] In some embodiments, the air-cooling temperature is 15-18°C, and the operating frequency of the cooling fan is greater than or equal to 45Hz.

[0051] Another embodiment of this application provides a packaging bag, which is made using the high-strength PE film obtained in the above embodiments. For example, the inner layer of the PE film can be bent to heat-seal and bond in opposite directions to obtain the packaging bag.

[0052] Example 1:

[0053] This embodiment provides a high-strength PE film, comprising a three-layer co-extruded layer formed by three-layer co-extrusion blown film, wherein the three-layer co-extruded layer includes an inner layer, a middle layer, and an outer layer. By weight percentage, the inner layer comprises 60% MLLDPE, 5% EVA, 29.5% LLDPE, and 0.5% PPA; by weight percentage, the middle layer comprises 65% MLLDPE, 14.5% LDPE, 20% LLDPE, 0.5% PPA, and 5% white masterbatch LE8236; and by weight percentage, the outer layer comprises 65% MLLDPE, 14.5% LDPE, 20% LLDPE, and 0.5% PPA.

[0054] The MLLDPE is model 1018MF (exxonMobil), the EVA is model 3172Z (DuPont), the LDPE is model 2426K (Maoming Petrochemical), and the PPA is model A1058 (a product of Beijing Yalen Zhilian Technology Co., Ltd.). In the inner layer, the LLDPE is model 1002BU (exxonMobil), and in the middle and outer layers, the LLDPE is model 7042 (Maoming Petrochemical). The white masterbatch is model LE8236 (brand or manufacturer: Guangdong Yilong New Material Technology Co., Ltd.).

[0055] The thickness of the inner layer is 33% of the total thickness of the film, the thickness of the middle layer is 33% of the total thickness of the film, and the thickness of the outer layer is 34% of the total thickness of the film. Specifically, for example, in a blown film of 100µm, the thickness of the inner layer is 33µm, the thickness of the middle layer is 33µm, and the thickness of the outer layer is 34µm. The preparation method of the PE film in this embodiment includes the following steps:

[0056] After the components of the inner layer are mixed evenly, they are fed into the inner layer hopper of the three-layer co-extrusion blown film machine.

[0057] After the components of the middle layer are mixed evenly, they are fed into the middle layer hopper of the three-layer co-extrusion blown film machine.

[0058] After the components of the outer layer are mixed evenly, they are fed into the outer hopper of the three-layer co-extrusion blown film machine.

[0059] The three-layer co-extrusion blown film mill melts and extrudes the components in each hopper onto the die, where they are blown into the PE film. The inner screw barrel temperature is 185°C. The middle screw barrel temperature is 190°C. The outer screw barrel temperature is 180°C. The die runner temperature is 185°C. The blow-up ratio is 3.0. The air-cooling temperature is 15°C. The die opening temperature is 185°C. The cooling fan operates at a frequency of 45Hz.

[0060] Example 2:

[0061] The PE film provided in this embodiment differs from the PE film provided in Embodiment 1 in that, by weight percentage, the inner layer comprises 70% MLLDPE, 5% EVA, 24.5% LLDPE, and 0.5% PPA; the middle layer comprises 70% MLLDPE, 10.5% LDPE, 15% LLDPE, 0.5% PPA, and 4% white masterbatch; and the outer layer comprises 70% MLLDPE, 11.5% LDPE, 18% LLDPE, and 0.5% PPA.

[0062] The preparation method in this embodiment differs from that in Example 1 in that the inner screw barrel temperature is 180°C, the middle screw barrel temperature is 195°C, the outer screw barrel temperature is 175°C, and the die head runner temperature is 190°C.

[0063] This application tests the properties of the PE film using the following method:

[0064] 1. Test tensile strength:

[0065] The test was conducted in accordance with GB / 1040.3. The test specimen was a long strip with a length of ≥150 mm and a width of 15 mm. The no-load speed was 250±25 m / min. The tensile force was the maximum load at which the specimen broke. The results were expressed as the average of 5 specimens in each group, with two significant figures.

[0066] 2. Test heat sealability

[0067] Tested according to the QB / T2358 standard.

[0068] 3. Drop test: 1.5 meters free fall, 6 drops, 2 drops on each side.

[0069] The test results of the above embodiments of this application are shown in the table below.

[0070]

[0071] In this application, by adjusting the PE formulation, the composite PE film has good tensile strength, good heat-sealing performance, good impact resistance, and high compressive strength.

[0072] The above embodiments are merely preferred embodiments of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-substantial changes and substitutions made by those skilled in the art based on the present invention shall fall within the scope of protection claimed by the present invention.

Claims

1. A high-strength PE film, comprising three co-extruded layers formed by three-layer co-extruded blown film, wherein the three co-extruded layers include an inner layer, a middle layer and an outer layer, It is characterized in that The inner layer comprises MLLDPE, EVA, LLDPE and PPA, the middle layer comprises MLLDPE, LDPE, LLDPE and PPA, and the outer layer comprises MLLDPE, LDPE, LLDPE and PPA.

2. The high-strength PE film according to claim 1, Features: The components of the inner layer are as follows in weight percentage: The components of the middle layer are as follows by weight percentage: The components of the outer layer are as follows by weight percentage:

3. The high-strength PE film according to claim 2, It is characterized in that The model of the MLLDPE is 1018MF, the model of the EVA is 3172Z, the model of the LDPE is 2426K, the model of the PPA is A1058, the model of the LLDPE in the inner layer is 1002BU, and the model of the LLDPE in the middle layer and the outer layer is 7042.

4. The high-strength PE film according to claim 2, It is characterized in that Calculated by weight percentage, the components of the middle layer also include 3%-5% of white masterbatch, and the model of the white masterbatch is LE8236.

5. The high-strength PE film according to claim 4, It is characterized in that The thickness of the inner layer is 33% of the total thickness of the film, the thickness of the middle layer is 33% of the total thickness of the film, and the thickness of the outer layer is 34% of the total thickness of the film.

6. A method for preparing a high-strength PE film, It is characterized in that The preparation method uses the components of each layer of the high-strength PE film according to any one of claims 1 to 5, and the preparation method comprises the following steps: The components of the inner layer are mixed evenly and then put into the inner layer hopper of the three-layer co-extrusion film blowing machine; The components of the middle layer are mixed evenly and then put into the middle layer hopper of the three-layer co-extrusion film blowing machine; The components of the outer layer are mixed evenly and then put into the outer layer hopper of the three-layer co-extrusion film blowing machine; Each extrusion screw of the three-layer co-extrusion film blowing machine melts and extrude the components in each hopper to the die head to blow into the PE film.

7. The preparation method according to claim 6, It is characterized in that The temperature of the inner screw barrel is 175-185°C, the temperature of the middle screw barrel is 185-195°C, the temperature of the outer screw barrel is 175-180°C, the flow channel temperature of the die head is 185-190°C, and the die mouth temperature is 185°C.

8. The preparation method according to claim 7, It is characterized in that The blowing ratio is 2.5-3.

0.

9. The preparation method according to claim 8, It is characterized in that The air cooling temperature is 15-18℃, and the operating frequency of the cooling fan is greater than or equal to 45Hz.

10. A packaging bag, It is characterized in that It is prepared using the high-strength PE film as described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Three-layer coextrusion heavy packaging membrane and fabrication method thereof

    CN103029388A

  • High-tensile cold drawing film and preparation method thereof

    CN109094163A

  • Composite film as well as preparation method and application thereof

    CN114801385A

  • Packaging film without fuzzing in bag making and manufacturing method thereof

    CN114801388A

  • Polyethylene film for medicine packaging and preparation method thereof

    CN116330785A