Optimized preparation and rapid detection method of carbon foam wave-absorbing material for wave-absorbing box
By introducing sheet boron nitride powder into the carbon foam and using spring probe method to detect, the problems of low thermal conductivity and cumbersome detection of carbon foam absorbing materials in the absorbing box are solved, and more efficient preparation and detection are achieved. Improves its performance and application range in the absorber box.
Patent Information
- Application Number
- CN202411044119.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-26
Smart Images

Figure CN119018876A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a batch preparation and application technology of absorbing materials suitable for a darkroom environment of an absorbing box, and specifically to an optimized preparation and rapid detection method of a carbon foam absorbing material for an absorbing box, and belongs to the field of material engineering. Background Art
[0002] The development of communication technology is becoming more and more important in the current military and civilian fields. Communication technology has been widely used in aerospace, military radar, electronic information, rail transportation, unmanned driving, intelligent robots and other fields. Electromagnetic signal transceiver antennas are key components in communication equipment. In order to accurately test and evaluate the electromagnetic performance of communication antennas, it is necessary to establish an extremely low scattering darkroom environment.
[0003] In recent years, my country has developed rapidly in the field of high technology, such as the gradual advancement of deep space exploration such as Tianwen, Tiangong and Chang'e projects, the extensive use of hypersonic aircraft, missiles and other hypersonic weapons, and the coverage of 5G communications in high-altitude and desert environments. For the above-mentioned application areas, it is no longer feasible to test and evaluate the electromagnetic performance of communication antennas in a conventional darkroom environment. It is necessary to create an extremely low-scattering absorbing box darkroom environment, and form various actual extreme use environments such as high temperature, ultra-low temperature, high vacuum, strong particle irradiation, and high-power antenna radiation in the box to accurately test the electromagnetic performance of communication antennas in actual use environments.
[0004] Therefore, it is particularly necessary to develop efficient anechoic chamber materials suitable for the extreme use environment of absorbing boxes and to prepare them in batches. In the previous work, the Institute of Metal Research of the Chinese Academy of Sciences developed carbon foam absorbing materials, that is, using amorphous silicon carbide powder and polymer materials as basic raw materials, foam resin as template, and preparing carbon foam absorbing materials through template hanging and pyrolysis process, and carried out the correlation study between the electrical conductivity of carbon foam and its absorbing performance. The carbon foam absorbing material can withstand the extreme use environment of various absorbing boxes and has the ability to produce in small batches. The Institute of Metal Research has also carried out relevant technical research on its application absorbing boxes. However, there are still two major technical difficulties in using the carbon foam developed in the early stage in the absorbing box: first, the thermal conductivity of the carbon foam developed in the early stage is relatively low (<0.45W / K·m). In order to meet the requirements of radiation heat dissipation and rapid temperature change of high-power antenna in the box, the carbon foam preparation process needs to be further optimized to significantly improve its thermal conductivity; second, in the process of conventional voltammetry to measure the conductivity of carbon foam through a fixture to check its electromagnetic properties, it is necessary to perform multiple operation steps such as edge machining of carbon foam materials, size measurement of carbon foam materials, and clamp tightness. The cumbersome operation steps restrict the detection speed and reduce the mass preparation capacity of carbon foam. It is necessary to propose a new method that can quickly detect the electromagnetic properties of carbon foam. Summary of the invention
[0005] The purpose of the present invention is to provide an optimized preparation and rapid detection method of carbon foam absorbing material for absorbing box, by which carbon foam absorbing material that is better suitable for the use environment of absorbing box can be prepared, and the technical bottleneck problem of batch preparation of carbon foam absorbing material can be effectively solved.
[0006] The technical solution of the present invention is:
[0007] The invention discloses an optimized preparation and rapid detection method of a carbon foam absorbing material for an absorbing box. The method uses flaky boron nitride powder and a polymer material as basic raw materials and a foam resin as a template. The carbon foam absorbing material is prepared by hanging and pyrolysis to prepare a carbon foam absorbing material with high conductivity and high dielectric loss. Based on the correlation between the electrical conductivity of the carbon foam and its absorbing performance, a spring probe method is used to test the two-point contact resistance value of the carbon foam to achieve rapid detection and screening of its electromagnetic performance.
[0008] The optimized preparation and rapid detection method of the carbon foam absorbing material for the absorbing box, the optimized preparation and detection process are as follows:
[0009] (1) Slurry preparation
[0010] The flaky boron nitride powder, polymer material, curing agent and ethanol are mixed in a certain proportion, ball milled after mechanical stirring, and filtered to obtain a slurry solution, wherein the weight content of the solute in the slurry solution is 5-60%; the weight percentage of the flaky boron nitride powder, polymer material and curing agent is 20-69wt%: 30-74wt%: 1-6wt%;
[0011] (2) Hanging molding
[0012] Cut polyurethane foam or polyether foam into required shapes and sizes, immerse them evenly in the slurry, remove excess slurry by air blowing or centrifugation, heat and semi-cure, repeat for many times until the foam precursor reaches the required specific gravity, and obtain a flake boron nitride reinforced resin foam precursor; the semi-curing conditions are 30-100°C and the time is 1-30 minutes;
[0013] (3) Hot pressing and densification
[0014] Put the flake boron nitride reinforced resin foam precursor into a high-pressure container, fill it with nitrogen or argon gas, and solidify it at high temperature and high pressure to obtain a dense boron nitride reinforced resin foam precursor; the pressure is 5 to 22 MPa, the temperature is 100 to 300°C, the heating rate is 1 to 5°C per minute, and the insulation time is 0.5 to 2 hours;
[0015] (4) Batch pyrolysis
[0016] The dense boron nitride reinforced resin foam precursor is charged into a furnace in large quantities for pyrolysis under argon, nitrogen or vacuum conditions, with a heating rate of 1 to 4°C per minute, and the temperature is raised to 600 to 800°C, and the temperature is kept for 5 minutes to 2 hours. The content of pyrolytic carbon graphitized microcrystals is controlled by temperature control, so as to control the electrical conductivity and electromagnetic properties of the pyrolytic carbon foam as a whole;
[0017] (5) Rapid testing
[0018] The spring probe method is used to quickly test the two-point contact resistance value of pyrolytic carbon foam. The electromagnetic properties of the carbon foam are judged by the corresponding relationship between the two-point contact resistance value and the electrical conductivity, and rapid screening and classification are achieved.
[0019] The optimized preparation and rapid detection method of the carbon foam absorbing material for the absorbing box, the flaky boron nitride powder used is hexagonal boron nitride, graphite-like layered structure, the boron nitride powder flake thickness is required to be 1-3μm, and the large surface particle size is required to be 10-60μm.
[0020] The optimized preparation and rapid detection method of the carbon foam absorbing material for the absorbing box, the spring probe detection device used in the spring probe method is assembled by two metal rods and two springs in two pen tubes, including a wire, an adhesive tape, a pen tube tail cover, a spring, a pad, a disc-shaped metal table, a metal rod, and a pen tube, as follows:
[0021] Each metal rod is respectively inserted into a pen tube, and one end of the metal rod passes through the head of the pen tube. A pen tube tail cap is installed at the tail of each pen tube, and the other end of the metal rod passes through the pen tube tail cap at the tail of the pen tube. The two metal rods are vertically welded with a disc-shaped metal platform at the same position when entering the pen tube. A spring is mounted on the metal rod between the disc-shaped metal platform and the pen tube tail cap. The two pen tube tail caps are respectively tightened and installed at the corresponding pen tube tails by screwing. The metal rod is pulled upward to make the spring just stressed, and then tape is wrapped around the part of the metal rod just exposed from the pen tube tail cap to fix it. The two assembled pen tubes are tied together in parallel with tape, and pads of different thicknesses are wedged between the two pen tubes to adjust the distance D between the two metal rods passing through the head of the pen tube. The two metal rods passing through the pen tube tail cap are welded to one end of two wires connected to the resistor to complete the preparation of the spring probe detection device.
[0022] The optimized preparation and rapid detection method of the carbon foam absorbing material for the absorbing box is as follows: the parts of the two metal rods passing through the head of the pen tube are used as "probes", and the diameter d and length L of the two probes are the same; the two metal rods are made of the same material, and the material is bronze, carbon steel or stainless steel; the two pen tubes are made of the same hard plastic material and have the same structural dimensions; the two springs are made of the same material and have the same length m and stiffness coefficient k.
[0023] The optimized preparation and rapid detection method of the carbon foam absorbing material for the absorbing box requires that the diameter d of the two probes is 1.5 mm to 4 mm, the length L of the two probes is 5 mm to 20 mm, and the distance D between the two probes is 10 mm to 30 mm; the length m of the two springs is 20 mm to 50 mm, and the stiffness coefficient k of the two springs is 500 N / m to 3000 N / m.
[0024] The optimized preparation and rapid detection method of the carbon foam absorbing material for the absorbing box is to select the d, L, D, m and k values of the spring probe detection device, that is, to determine the distance between the two points of the probe and the contact pressure, firstly connect the two wires connected to the metal rod to the positive and negative poles of the resistance meter respectively, then contact the two probes with the carbon foam tendons, and apply pressure until the two probes are pressed into the pen tube, so as to quickly measure the contact resistance value of the two points of the carbon foam.
[0025] The optimized preparation and rapid detection method of the carbon foam absorbing material for the absorbing box shows different electromagnetic properties for carbon foam absorbing materials with different conductivity, establishes a corresponding relationship between different two-point contact resistance values and different conductivity, and then quickly clarifies its electromagnetic properties by measuring the two-point contact resistance value of the carbon foam, thereby achieving rapid screening.
[0026] The design concept of the present invention is:
[0027] The present invention is based on amorphous silicon carbide powder and polymer materials as basic raw materials, foam resin as template, and the preliminary work of hanging and pyrolysis to prepare carbon foam absorbing materials. Hexagonal flaky boron nitride powder is used to replace amorphous silicon carbide powder. Hexagonal boron nitride can form a graphite-like lamellar structure, also known as "white graphite". For hexagonal lamellar boron nitride, like graphite, it has extremely high thermal conductivity (300W / K·m~2000W / K·m) in the lamellar direction. In the precursor hanging operation, with the help of the flow and centrifugal effect of the polymer resin, the hexagonal boron nitride lamellae can be laid out along the foam tendons, so that the high thermal conductivity of the hexagonal boron nitride lamellae direction can be fully utilized, and the thermal conductivity of the carbon foam absorbing material can be greatly improved, making it better suitable for the darkroom use environment of the absorbing box. In addition, the real part of the dielectric constant ε' of hexagonal boron nitride is smaller than that of silicon carbide. When the imaginary part ε" of the dielectric constant of carbon foam with the same conductivity does not change much, the dielectric loss (ε" / ε') of the carbon foam increases after the introduction of hexagonal boron nitride, which is beneficial to improving the microwave absorption performance of the pointed cone darkroom structure.
[0028] The present invention is based on the previous work foundation of the correlation between the conductivity of carbon foam and its wave absorbing performance, and adopts the spring probe method to quickly test the two-point contact resistance value of pyrolytic carbon foam. A spring probe detection device is made by assembling two metal rods and two springs in two pen tubes. On the premise of determining the distance between the two points of the probe and the pressure of contacting the carbon foam, the two-point contact resistance value of the carbon foam is tested under pressure. For carbon foam wave absorbing materials with different conductivities, different electromagnetic properties are exhibited, and the corresponding relationship between different two-point contact resistance values and different conductivities is established. Then, by measuring the two-point contact resistance value of the carbon foam, its electromagnetic properties are quickly clarified, and the technical bottleneck problem of mass preparation of carbon foam wave absorbing materials is effectively solved.
[0029] The present invention has the following advantages and beneficial effects:
[0030] 1. Significantly improved the environmental applicability of the carbon foam absorbing material in the absorbing box
[0031] The carbon foam absorbing material prepared by optimizing hexagonal flake boron nitride powder in the present invention is not only suitable for various extreme use environments in the absorbing box, but also, at the same volume fraction, the thermal conductivity can be increased by more than 1 times compared with the carbon foam absorbing material using amorphous silicon carbide powder, making it more suitable for the temperature control requirements of rapid heat dissipation and rapid temperature change of the absorbing box; in addition, the introduction of flake boron nitride can significantly improve the dielectric loss capacity of the carbon foam and enhance the absorbing performance of its pointed cone darkroom structure. The optimized prepared carbon foam can achieve the following beneficial effects: first, the improvement of the heat dissipation and rapid temperature change capacity of the carbon foam is conducive to increasing its arrangement thickness and arrangement quality in the absorbing box; second, the reduction of the real part ε' of the carbon foam dielectric constant and the significant increase of the dielectric loss (ε" / ε') are conducive to expanding the absorbing capacity of the pointed cone darkroom structure to a lower frequency band, and these effects will significantly improve the environmental adaptability and application range of the carbon foam in the absorbing box.
[0032] 2. Significantly improved the batch preparation capacity of carbon foam absorbing materials
[0033] The present invention adopts the two-point contact resistance value test of the spring probe method to realize the rapid classification of pyrolytic carbon foam absorbing materials. A large number of boron nitride enhanced resin foam precursors are loaded in the same pyrolysis furnace. The pyrolysis temperature control can only regulate the conductivity and electromagnetic properties of the pyrolytic carbon foam as a whole. However, each resin foam precursor has a different heating state and a different degree of pyrolysis due to its different placement, which makes the conductivity and electromagnetic properties of each resin foam precursor different. Therefore, it is necessary to quickly screen and classify carbon foams with different electromagnetic properties, so as to provide carbon foams with different electromagnetic properties in batches for absorbing boxes with different absorbing performance requirements. The spring probe method realizes the rapid screening of carbon foam absorbing materials with different electromagnetic properties, significantly improving the batch preparation capacity.
[0034] In summary, the present invention provides an optimized preparation and rapid detection method for carbon foam absorbing materials for absorbing boxes. The method prepares carbon foam absorbing materials that are more suitable for the use environment of absorbing boxes, and effectively solves the technical bottleneck problem of batch preparation, making carbon foam absorbing materials have a broader application prospect in the field of absorbing boxes. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the macroscopic morphology of the flake-shaped boron nitride powder carbon foam absorbing material.
[0036] Figure 2 The microscopic morphology (left) and partial enlarged image (right) of the flaky boron nitride powder carbon foam absorbing material. In the right image, a is pyrolytic carbon, b is flaky boron nitride.
[0037] Figure 3 The schematic diagram of the structure of the spring probe detection device is shown in the figure, 1 is a wire (connected to the resistor), 2 is a tape, 3 is a pen tube tail cap, 4 is a spring (stubborn system k), 5 is a cushion block, 6 is a disc-shaped metal platform, 7 is a metal rod, 8 is a pen tube, and 9 is a probe.
[0038] Figure 4 This is the corresponding relationship between the two-point contact resistance of carbon foam doped with flake boron nitride powder and the electrical conductivity of the foam.
[0039] Figure 5-Figure 12 The corresponding relationship between the two-point contact resistance value and electromagnetic performance of carbon foam doped with flake boron nitride powder. Figure 5 This is the frequency response curve of the dielectric constant of carbon foam with 1KΩ contact resistance; Figure 6 This is the frequency response curve of dielectric loss of carbon foam with 1KΩ contact resistance; Figure 7 This is the frequency response curve of dielectric constant of carbon foam with 3KΩ contact resistance; Figure 8 This is the frequency response curve of dielectric loss of carbon foam with 3KΩ contact resistance; Fig. 9 This is the frequency response curve of the dielectric constant of carbon foam with 5KΩ contact resistance; Fig.10 This is the frequency response curve of dielectric loss of carbon foam with 5KΩ contact resistance; Fig.11 This is the frequency response curve of dielectric constant of carbon foam with 9KΩ contact resistance; Fig.12 This is the frequency response curve of dielectric loss of carbon foam with 9KΩ contact resistance. DETAILED DESCRIPTION
[0040] In the specific implementation process, the present invention proposes an optimized preparation and rapid detection method for a carbon foam absorbing material for an absorbing box. Based on the preliminary work of using amorphous silicon carbide powder and polymer materials as basic raw materials and foam resin as a template to prepare carbon foam absorbing materials by hanging and pyrolysis, the optimized preparation method of the present invention is to replace amorphous silicon carbide powder with flaky boron nitride powder, which can significantly improve the thermal conductivity of carbon foam on the one hand, so as to improve its heat dissipation and temperature control capabilities in the absorbing box, and on the other hand, it can significantly increase the dielectric loss capacity of carbon foam to optimize the absorbing performance of its pointed cone darkroom structure, so that the carbon foam is better suitable for the use environment of the absorbing box; based on the preliminary work of the correlation between the electrical conductivity of carbon foam and its absorbing performance, the rapid detection method of the present invention is to use a spring probe method to test the two-point contact resistance of carbon foam. Under the premise of determining the distance between the two points of the probe and the contact pressure, the two-point contact resistance value test can realize the rapid detection and screening of the electromagnetic properties of a large number of carbon foams.
[0041] The present invention is further illustrated below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0042] Example 1
[0043] In this embodiment, flaky boron nitride powder (lamella thickness 3 μm, average particle size 60 μm), phenol-formaldehyde resin and curing agent (p-toluenesulfonic acid) in a weight ratio of 52%:42%:6% are mixed in anhydrous ethanol to prepare a slurry (solute content 30 wt%), and polyurethane foam is cut into 40 pieces of 220 mm × 220 mm × 55 mm in size, and immersed in the slurry respectively. After being taken out, the excess slurry is removed by centrifugation, and semi-curing is carried out at 60°C for 10 minutes. This is repeated 17 times until the specific gravity of the foam precursor reaches 0.5 g / cm 3 , put it into a high-pressure container, fill it with nitrogen to make the air pressure reach 12MPa, heat it to 250℃ at 5℃ per minute, keep it warm for 1 hour to solidify, then divide 40 foam precursors into 8 stacks, and put 5 pieces in each stack into the pyrolysis furnace for pyrolysis under argon protection, heat it to 750℃ at 2℃ per minute, and keep it warm for 0.5 hour.
[0044] In this embodiment, the thermal conductivity of the prepared carbon foam is between 0.94W / K·m and 1.12W / K·m. A spring probe detection device with a probe diameter of d=2mm, a probe length of L=10mm, a probe spacing of D=15mm, a spring length of m=35mm, and a spring stiffness coefficient of k=1500N / m is used to quickly test the two-point contact resistance value R of the carbon foam, including 8 pieces of carbon foam with 1KΩ≤R≤2KΩ, 6 pieces of carbon foam with 2KΩ<R≤3KΩ, 10 pieces of carbon foam with 3KΩ<R≤5KΩ, 6 pieces of carbon foam with 5KΩ<R≤7KΩ, 8 pieces of carbon foam with 7KΩ<R≤9KΩ, and 2 pieces of carbon foam with 9KΩ<R≤13KΩ. The prepared carbon foam can be used as an absorbing material for different absorbing boxes.
[0045] like Figure 1 As shown, from the macroscopic morphology of the flaky boron nitride powder carbon foam absorbing material, it can be seen that the carbon foam has uniform pore size, a continuous matrix, and no obvious defects.
[0046] like Figure 2 As shown, from the microscopic morphology of the carbon foam absorber using flaky boron nitride powder, it can be seen that the hexagonal boron nitride flakes are laid flat along the foam ribs, which can give full play to the high thermal conductivity of the hexagonal boron nitride flakes and greatly improve the thermal conductivity of the carbon foam absorber.
[0047] like Figure 3 As shown in the figure, the structural schematic diagram of the spring probe detection device used in Example 1 is adopted. In the following embodiments, the spring probe detection device with the same structural dimensions as that of Example 1 is adopted. The spring probe detection device is assembled by two metal rods 7 and two springs 4 in two pen tubes 8, and mainly includes a wire 1, an adhesive tape 2, a pen tube tail cover 3, a spring 4, a pad 5, a disc-shaped metal platform 6, a metal rod 7, a pen tube 8, and a probe 9, which are specifically as follows:
[0048] Each metal rod 7 is respectively inserted into a pen tube 8, one end of the metal rod 7 passes through the head of the pen tube 8, a pen tube tail cover 3 is installed at the tail of each pen tube 8, and the other end of the metal rod 7 passes through the pen tube tail cover 3 at the tail of the pen tube 8. The two metal rods 7 are vertically welded with a disc-shaped metal platform 6 at the same position where they enter the pen tube 8. A spring 4 is mounted on the metal rod 7 between the disc-shaped metal platform 6 and the pen tube tail cover 3. The two pen tube tail covers 3 are respectively tightened and installed at the tail of the corresponding pen tube 8 by screwing. The metal rod 7 is pulled upward to make the spring 4 just stressed, and then the tape 2 is wrapped around the part of the metal rod 7 just exposed from the pen tube tail cover 3 to fix it. The two assembled pen tubes 8 are parallelly tied together with the tape 2. A pad 5 of different thicknesses can be wedged between the two pen tubes 8 to adjust the distance D between the two metal rods 7 passing through the head of the pen tube 8. The two metal rods 7 that pass through the pen tube tail cover 3 are welded to one end of two wires 1 connected to the resistor, so that the preparation of the spring probe detection device is completed. The two metal rods 7 that pass through the head of the pen tube 8 are used as "probes 9", and the diameter d and length L of the two probes 9 are the same. The two metal rods 7 are made of the same material, which can be bronze, carbon steel or stainless steel. The two pen tubes 8 are made of the same hard plastic material and have the same structural dimensions. The two springs 4 are made of the same material and have the same length m and stiffness coefficient k.
[0049] The diameter d of the two probes is required to be 1.5mm-4mm, the length L of the two probes is required to be 5mm-20mm, and the distance D between the two probes is required to be 10mm-30mm; the length m of the two springs is required to be 20mm-50mm, and the stiffness coefficient k of the two springs is required to be 500N / m-3000N / m. Prepare and fix the d, L, D, m and k values of the spring probe detection device, that is, on the premise of determining the distance between the two points of the probe and the contact pressure, first connect the two wires 1 connecting the metal rod 7 to the positive and negative poles of the resistance meter respectively, then contact the two probes 9 on the carbon foam tendons, and apply pressure until the two probes 9 are pressed into the pen tube 8, so that the two-point contact resistance value of the carbon foam can be quickly measured.
[0050] like Figure 4 As shown, from the corresponding relationship between the two-point contact resistance value of carbon foam and the foam conductivity measured by the spring probe detection device in Example 1, it can be seen that the larger the two-point contact resistance value R, the smaller the conductivity, and vice versa.
[0051] like Figure 5-Figure 12As shown, from the corresponding relationship between the two-point contact resistance value of the carbon foam and the electromagnetic performance measured by the spring probe detection device in Example 1, it can be seen that different two-point contact resistance values correspond to different foam conductivities, and also correspond to different frequency-response electromagnetic parameters: the smaller the two-point contact resistance value R, the larger the frequency-response dielectric constant of the carbon foam, and the larger the frequency-response dielectric loss. If R<1KΩ, the carbon foam reflects too much electromagnetic waves and is not suitable as an absorbing material; the larger the two-point contact resistance value R, the smaller the frequency-response dielectric constant of the carbon foam, and the smaller the frequency-response dielectric loss. If R>13KΩ, the carbon foam transmits too much electromagnetic waves and is not suitable as an absorbing material.
[0052] Example 2
[0053] In this embodiment, flaky boron nitride powder (flaky thickness 2 μm, average particle size of large surface 45 μm), epoxy resin (brand EP0141-310) and curing agent (p-toluenesulfonic acid) in a weight ratio of 35%:60%:5% are mixed in anhydrous ethanol to prepare a slurry (solute content is 40wt%), and polyurethane foam is cut into 50 pieces of 240mm×240mm×45mm size, immersed in the slurry respectively, and then taken out by centrifugation to remove excess slurry, semi-cured at 80°C for 5 minutes, and repeated 13 times until the specific gravity of the foam precursor reaches 0.43g / cm 3 , put it into a high-pressure container, fill it with nitrogen to make the air pressure reach 10MPa, heat it to 200℃ at 2℃ per minute, keep it warm for 1 hour to solidify, then divide 50 foam precursors into 10 stacks, and put 50 foam precursors in each stack into a pyrolysis furnace for pyrolysis under argon protection, heat it to 800℃ at 3℃ per minute, and keep it warm for 5 minutes.
[0054] In this embodiment, the thermal conductivity of the prepared carbon foam is between 1.2W / K·m and 1.3W / K·m. The spring probe detection device used in Example 1 is used to quickly test the two-point contact resistance value R of the carbon foam, including 4 pieces of carbon foam with R<1KΩ, 20 pieces of carbon foam with 1KΩ≤R≤2KΩ, 10 pieces of carbon foam with 2KΩ<R≤3KΩ, 10 pieces of carbon foam with 3KΩ<R≤5KΩ, and 6 pieces of carbon foam with 5KΩ<R≤7KΩ. The 4 pieces of carbon foam with R<1KΩ cannot be used as absorbing materials because of their large dielectric constant and dielectric loss. The remaining 46 pieces of carbon foam can be used as absorbing materials for different absorbing boxes.
[0055] Example 3
[0056] In this embodiment, flaky boron nitride powder (flaky thickness 1.5 μm, average particle size of large surface 30 μm), boron phenolic resin and curing agent (urotropine) in a weight ratio of 52%:44%:4% are mixed in anhydrous ethanol to prepare a slurry (solute content 30wt%), and polyurethane foam is cut into 40 pieces of 240mm×240mm×50mm size, immersed in the slurry respectively, and then taken out by centrifugation to remove excess slurry, semi-cured at 60°C for 20 minutes, and repeated 13 times until the specific gravity of the foam precursor reaches 0.41g / cm 3 , put it into a high-pressure container, fill it with nitrogen to make the air pressure reach 18MPa, heat it to 260℃ at 4℃ per minute, keep it warm for 0.5 hours to solidify, then divide 40 foam precursors into 8 stacks, and load 5 pieces in each stack into the pyrolysis furnace for pyrolysis under argon protection, heat it to 610℃ at 2℃ per minute, and keep it warm for 2 hours.
[0057] In this embodiment, the thermal conductivity of the prepared carbon foam is between 0.72W / K·m and 0.77W / K·m. The spring probe detection device used in Example 1 is used to quickly test the two-point contact resistance value R of the carbon foam, including 8 pieces of carbon foam with 5KΩ<R≤7KΩ, 12 pieces of carbon foam with 7KΩ<R≤9KΩ, 16 pieces of carbon foam with 9KΩ<R≤13KΩ, and 4 pieces of carbon foam with R>13KΩ. The 4 pieces of carbon foam with R>13KΩ cannot be used as absorbing materials because of their too small dielectric constant and dielectric loss. The remaining 36 pieces of carbon foam can be used as absorbing materials for different absorbing boxes.
[0058] Example 4
[0059] In this embodiment, flaky boron nitride powder (flaky thickness 2 μm, average particle size of large surface 45 μm), furfural resin and curing agent (urotropine) in a weight ratio of 24%:71%:5% are mixed in anhydrous ethanol to prepare a slurry (solute content is 50wt%), and polyurethane foam is cut into 120 pieces of 220mm×220mm×20mm size, and immersed in the slurry respectively. After taking out, the excess slurry is removed by centrifugation, and semi-curing is carried out at 90°C for 5 minutes, which is repeated 12 times until the specific gravity of the foam precursor reaches 0.48g / cm 3 , put it into a high-pressure container, fill it with nitrogen to make the air pressure reach 15MPa, heat it to 240℃ at 2℃ per minute, keep it warm for 1 hour to solidify, then divide 120 foam precursors into 10 stacks, and put 12 pieces in each stack into the pyrolysis furnace for pyrolysis under argon protection, heat it to 690℃ at 2℃ per minute, and keep it warm for 35 minutes.
[0060] In this embodiment, the thermal conductivity of the prepared carbon foam is between 0.69W / K·m and 0.75W / K·m. The spring probe detection device used in Example 1 is used to quickly test the two-point contact resistance value R of the carbon foam, including 10 pieces of carbon foam with 1KΩ≤R≤2KΩ, 28 pieces of carbon foam with 2KΩ<R≤3KΩ, 12 pieces of carbon foam with 3KΩ<R≤5KΩ, 28 pieces of carbon foam with 5KΩ<R≤7KΩ, 34 pieces of carbon foam with 7KΩ<R≤9KΩ, and 8 pieces of carbon foam with 9KΩ<R≤13KΩ. The prepared carbon foam can be used as an absorbing material for different absorbing boxes.
[0061] Example 5
[0062] In this embodiment, flaky boron nitride powder (lamella thickness 3 μm, average particle size 60 μm), phenol-formaldehyde resin and curing agent (p-toluenesulfonic acid) in a weight ratio of 45%:50%:5% are mixed in anhydrous ethanol to prepare a slurry (solute content is 45wt%), and polyurethane foam is cut into 60 pieces of 220mm×220mm×35mm size, immersed in the slurry respectively, and then taken out by centrifugation to remove excess slurry, semi-cured at 70°C for 10 minutes, and repeated 14 times until the specific gravity of the foam precursor reaches 0.45g / cm 3 , put it into a high-pressure container, fill it with nitrogen to make the air pressure reach 20MPa, heat it to 280℃ at 5℃ per minute, keep it warm for 1 hour to solidify, then divide 60 foam precursors into 10 stacks, and load 6 pieces in each stack into the pyrolysis furnace for pyrolysis under argon protection, heat it to 720℃ at 2℃ per minute, and keep it warm for 25 minutes.
[0063] In this embodiment, the thermal conductivity of the prepared carbon foam is between 0.88W / K·m and 0.96W / K·m. The spring probe detection device used in Example 1 is used to quickly test the two-point contact resistance value R of the carbon foam, including 14 pieces of carbon foam with 1KΩ≤R≤2KΩ, 12 pieces of carbon foam with 2KΩ<R≤3KΩ, 12 pieces of carbon foam with 3KΩ<R≤5KΩ, 10 pieces of carbon foam with 5KΩ<R≤7KΩ, 8 pieces of carbon foam with 7KΩ<R≤9KΩ, and 4 pieces of carbon foam with 9KΩ<R≤13KΩ. The prepared carbon foam can be used as an absorbing material for different absorbing boxes.
[0064] Example 6
[0065] The difference from Example 5 is that flaky boron nitride powder with a layer thickness of 1 μm and a large-surface average particle size of 20 μm is used.
[0066] In this embodiment, the thermal conductivity of the prepared carbon foam is between 0.71W / K·m and 0.83W / K·m. The spring probe detection device used in Example 1 is used to quickly test the two-point contact resistance value R of the carbon foam, wherein 10 pieces of carbon foam with 1KΩ≤R≤2KΩ, 10 pieces of carbon foam with 2KΩ<R≤3KΩ, 12 pieces of carbon foam with 3KΩ<R≤5KΩ, 12 pieces of carbon foam with 5KΩ<R≤7KΩ, 12 pieces of carbon foam with 7KΩ<R≤9KΩ, and 4 pieces of carbon foam with 9KΩ<R≤13KΩ. The prepared carbon foam can be used as an absorbing material for different absorbing boxes.
[0067] Example 7
[0068] The difference from Example 5 is that the solute content of the slurry is 8wt%, and the material needs to be hung 35 times until the specific gravity of the foam precursor reaches 0.45g / cm 3 .
[0069] In this embodiment, the thermal conductivity of the prepared carbon foam is between 0.92W / K·m and 0.98W / K·m. The spring probe detection device used in Example 1 is used to quickly test the two-point contact resistance value R of the carbon foam, including 14 pieces of carbon foam with 1KΩ≤R≤2KΩ, 12 pieces of carbon foam with 2KΩ<R≤3KΩ, 12 pieces of carbon foam with 3KΩ<R≤5KΩ, 10 pieces of carbon foam with 5KΩ<R≤7KΩ, 8 pieces of carbon foam with 7KΩ<R≤9KΩ, and 4 pieces of carbon foam with 9KΩ<R≤13KΩ. The prepared carbon foam can be used as an absorbing material for different absorbing boxes.
[0070] Example 8
[0071] The difference from Example 5 is that the pyrolysis temperature is 650° C. and the temperature is maintained for 1 hour.
[0072] In this embodiment, the thermal conductivity of the prepared carbon foam is between 0.79W / K·m and 0.91W / K·m. The spring probe detection device used in Example 1 is used to quickly test the two-point contact resistance value R of the carbon foam, including 14 pieces of carbon foam with 3KΩ<R≤5KΩ, 10 pieces of carbon foam with 5KΩ<R≤7KΩ, 10 pieces of carbon foam with 7KΩ<R≤9KΩ, 20 pieces of carbon foam with 9KΩ<R≤13KΩ, and 6 pieces of carbon foam with R>13KΩ. The 6 pieces of carbon foam with R>13KΩ cannot be used as absorbing materials because of their too small dielectric constant and dielectric loss. The remaining 54 pieces of carbon foam can be used as absorbing materials for different absorbing boxes.
[0073] Example 9
[0074] The difference from Example 5 is that the pyrolysis temperature is 770°C and the temperature is kept for 15 minutes.
[0075] In this embodiment, the thermal conductivity of the prepared carbon foam is between 0.93W / K·m and 1.09W / K·m. The spring probe detection device used in Example 1 is used to quickly test the two-point contact resistance value R of the carbon foam, including 4 pieces of carbon foam with R<1KΩ, 20 pieces of carbon foam with 1KΩ≤R≤2KΩ, 10 pieces of carbon foam with 2KΩ<R≤3KΩ, 10 pieces of carbon foam with 3KΩ<R≤5KΩ, 10 pieces of carbon foam with 5KΩ<R≤7KΩ, and 6 pieces of carbon foam with 7KΩ<R≤9KΩ. The 4 pieces of carbon foam with R<1KΩ cannot be used as absorbing materials because of their large dielectric constant and dielectric loss. The remaining 56 pieces of carbon foam can be used as absorbing materials for different absorbing boxes.
[0076] The implementation results show that the present invention addresses two major technical difficulties that still exist in the prior art when using carbon foam in microwave absorbing boxes, and proposes two new methods: one is to introduce hexagonal flake boron nitride powder to replace amorphous silicon carbide powder, which can not only significantly improve the thermal conductivity of the carbon foam but also increase the dielectric loss capacity of the carbon foam, making the carbon foam better suitable for the use environment of the microwave absorbing box; the second is to adopt the spring probe method to test the two-point contact resistance value of the carbon foam to correspond to its electrical conductivity and electromagnetic properties, thereby realizing rapid detection and solving the technical bottleneck problem of mass preparation of carbon foam absorbing materials.
Claims
1. An optimized preparation and rapid detection method of carbon foam absorbing material for absorbing box, characterized in that: Using flaky boron nitride powder and polymer materials as basic raw materials and foam resin as template, carbon foam absorbing materials are prepared by hanging and pyrolysis, and carbon foam absorbing materials with high conductivity and high dielectric loss are prepared; based on the correlation between the electrical conductivity of carbon foam and its absorbing performance, the spring probe method is used to test the two-point contact resistance value of carbon foam to achieve rapid detection and screening of its electromagnetic properties.
2. The optimized preparation and rapid detection method of carbon foam absorbing material for absorbing box according to claim 1, characterized in that: The optimized preparation and detection process is as follows: (1) Slurry preparation The flaky boron nitride powder, polymer material, curing agent and ethanol are mixed in a certain proportion, ball milled after mechanical stirring, and filtered to obtain a slurry solution, wherein the weight content of the solute in the slurry solution is 5-60%; the weight percentage of the flaky boron nitride powder, polymer material and curing agent is 20-69wt%: 30-74wt%: 1-6wt%; (2) Hanging molding Cut polyurethane foam or polyether foam into required shapes and sizes, immerse them evenly in the slurry, remove excess slurry by air blowing or centrifugation, heat and semi-cure, repeat for many times until the foam precursor reaches the required specific gravity, and obtain a flake boron nitride reinforced resin foam precursor; the semi-curing conditions are 30-100°C and the time is 1-30 minutes; (3) Hot pressing and densification Put the flake boron nitride reinforced resin foam precursor into a high-pressure container, fill it with nitrogen or argon gas, and solidify it at high temperature and high pressure to obtain a dense boron nitride reinforced resin foam precursor; the pressure is 5 to 22 MPa, the temperature is 100 to 300°C, the heating rate is 1 to 5°C per minute, and the insulation time is 0.5 to 2 hours; (4) Batch pyrolysis The dense boron nitride reinforced resin foam precursor is charged into a furnace in large quantities for pyrolysis under argon, nitrogen or vacuum conditions, with a heating rate of 1 to 4°C per minute, and the temperature is raised to 600 to 800°C, and the temperature is kept for 5 minutes to 2 hours. The content of pyrolytic carbon graphitized microcrystals is controlled by temperature control, so as to control the electrical conductivity and electromagnetic properties of the pyrolytic carbon foam as a whole; (5) Rapid testing The spring probe method is used to quickly test the two-point contact resistance value of pyrolytic carbon foam. The electromagnetic properties of the carbon foam are judged by the corresponding relationship between the two-point contact resistance value and the electrical conductivity, and rapid screening and classification are achieved.
3. The optimized preparation and rapid detection method of carbon foam absorbing material for absorbing box according to claim 2, characterized in that: The flaky boron nitride powder used is hexagonal boron nitride with a graphite-like layered structure. The boron nitride powder flake thickness is required to be 1 to 3 μm, and the large surface particle size is required to be 10 to 60 μm.
4. The optimized preparation and rapid detection method of carbon foam absorbing material for absorbing box according to claim 2, characterized in that: The spring probe detection device used in the spring probe method is composed of two metal rods and two springs assembled in two pen tubes, including a wire, an adhesive tape, a pen tube tail cap, a spring, a pad, a disc-shaped metal table, a metal rod, and a pen tube, as follows: Each metal rod is respectively inserted into a pen tube, and one end of the metal rod passes through the head of the pen tube. A pen tube tail cap is installed at the tail of each pen tube, and the other end of the metal rod passes through the pen tube tail cap at the tail of the pen tube. The two metal rods are vertically welded with a disc-shaped metal platform at the same position when entering the pen tube. A spring is mounted on the metal rod between the disc-shaped metal platform and the pen tube tail cap. The two pen tube tail caps are respectively tightened and installed at the corresponding pen tube tails by screwing. The metal rod is pulled upward to make the spring just stressed, and then tape is wrapped around the part of the metal rod just exposed from the pen tube tail cap to fix it. The two assembled pen tubes are tied together in parallel with tape, and pads of different thicknesses are wedged between the two pen tubes to adjust the distance D between the two metal rods passing through the head of the pen tube. The two metal rods passing through the pen tube tail cap are welded to one end of two wires connected to the resistor to complete the preparation of the spring probe detection device.
5. The optimized preparation and rapid detection method of carbon foam absorbing material for absorbing box according to claim 4, characterized in that: The parts of the two metal rods that pass through the head of the pen tube serve as "probes", and the diameter d and length L of the two probes are the same; the two metal rods are made of the same material, which can be bronze, carbon steel or stainless steel; the two pen tubes are made of the same hard plastic material and have the same structural dimensions; the two springs are made of the same material and have the same length m and stiffness coefficient k.
6. The optimized preparation and rapid detection method of carbon foam absorbing material for absorbing box according to claim 4, characterized in that: The diameter d of the two probes is required to be 1.5mm~4mm, the length L of the two probes is required to be 5mm~20mm, and the distance D between the two probes is required to be 10mm~30mm; the length m of the two springs is required to be 20mm~50mm, and the stiffness coefficient k of the two springs is required to be 500N / m~3000N / m.
7. The optimized preparation and rapid detection method of carbon foam absorbing material for absorbing box according to claim 6, characterized in that: Select the d, L, D, m and k values of the spring probe detection device, that is, determine the distance between the two points of the probe and the contact pressure. First, connect the two wires connected to the metal rod to the positive and negative poles of the resistance meter respectively, and then contact the two probes with the carbon foam tendons. Apply pressure until the two probes are pressed into the pen tube, and quickly measure the contact resistance value of the two points of the carbon foam.
8. The optimized preparation and rapid detection method of carbon foam absorbing material for absorbing box according to claim 7, characterized in that: Carbon foam absorbing materials with different electrical conductivities exhibit different electromagnetic properties. A corresponding relationship between different two-point contact resistance values and different electrical conductivities is established, and then the electromagnetic properties of the carbon foam are quickly determined by measuring the two-point contact resistance values, thereby achieving rapid screening.
Citation Information
Patent Citations
Boron nitride foam material and preparation method thereof
CN109095930A
Preparation method of boron nitride / carbon foam material
CN114180972A
Compact foamy thyrite in high intensity and preparation method
CN1600742A
Test equipment of product resistance fast
CN206248725U
Magnetic material surface resistivity test pen
CN213779952U