Preparation method of biomass hard carbon lithium ion battery negative electrode material

The negative electrode material of biomass hard carbon lithium-ion battery is prepared through hydrothermal reaction and high-temperature carbonization. The hard carbon material with high-level spacing and active sites is formed by using rapeseed pollen and modifiers, which solves the problem of low efficiency of hard carbon materials and improves the battery electrochemical properties and reversible capacity.

CN119018879APending Publication Date: 2024-11-26SICHUAN HAICHUANG SHANGWEI NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411220289.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The first time the existing hard carbon has low efficiency and conductivity as the negative electrode material for lithium-ion batteries, and cannot meet the actual application needs.

Method used

Prepare the negative electrode material of biomass hard carbon lithium-ion battery through hydrothermal reaction and high-temperature carbonization, and use biomass raw materials such as rape pollen and modifiers such as phosphoric acid and phosphorous acid to form hard carbon materials with high layer spacing and active sites, thereby improving the Conductivity and first-time Coulomb efficiency.

Benefits of technology

It improves the electrochemical performance and reversible capacity of hard carbon materials, enhances the embedded/de-embedding capability of lithium ions, improves the charging performance of the battery, while maintaining high first-time Coulomb efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018879A_ABST
    Figure CN119018879A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a biomass hard carbon lithium ion battery negative electrode material, and relates to the field of battery technology research. Comprising the following steps: pretreating a biomass raw material to obtain a pretreated material; placing the pretreated material in a solution in which a modifier is dissolved, then stirring and dispersing, transferring into a stainless steel reaction kettle for reaction, and after the reaction is finished, carrying out centrifugal washing and filtering to obtain a modified material; and transferring the modified material into a tubular furnace, introducing shielding gas, and carrying out high-temperature carbonization to obtain the biomass hard carbon material. A plurality of active sites can be formed through the biomass raw material, the electrochemical performance of hard carbon is improved by increasing the interlayer space and improving the conductivity, and the first coulombic efficiency of the hard carbon material can be improved; the hydrothermal treatment method maintains the original morphology of the rape pollen, and the elliptical particles not only are beneficial to improving the stacking density of the material, but also endow the capacity and the first-effect improvement of the carbon material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology research, and in particular to a method for preparing a biomass hard carbon lithium ion battery negative electrode material. Background Art

[0002] At present, in order to reduce pollution and improve the environment, new energy vehicles have been developed rapidly and maintained a continuous growth trend. Among them, batteries play an extremely important role. Lithium-ion batteries are widely used due to their high energy density and long cycle life. Lithium-ion batteries are composed of negative electrodes, positive electrodes, electrolytes and separators, among which the negative electrode largely determines the key performance of lithium batteries. Therefore, the development of high-performance negative electrode materials has become one of the most important and urgent directions for lithium-ion batteries. At present, the negative electrode of commercial lithium-ion batteries is mainly made of graphite. Graphite has the advantages of high electronic conductivity, large lithium ion diffusion coefficient, small volume change of layered structure before and after lithium insertion, and low lithium insertion potential, but its low temperature resistance and rate performance restrict the effective operation of the battery. Compared with graphite, hard carbon not only has abundant micropores, but also forms short-range ordered but long-range disordered characteristics, which is conducive to the transfer of lithium ions and improves the rate performance. In addition, the larger interlayer spacing allows faster insertion / deinsertion of lithium ions, making it a suitable negative electrode material for fast charging of lithium-ion batteries. However, the first coulombic efficiency of hard carbon anode is low, which is far from meeting the needs of practical applications. Therefore, to meet the application of hard carbon in practical batteries, the main challenge is how to increase the reversible capacity without sacrificing the first coulombic efficiency.

[0003] The sources of hard carbon include resin, asphalt-based, biomass, etc. Among them, biomass materials have attracted extensive attention from researchers because of their renewable nature, low pollution, wide sources and low cost. The unique ellipsoidal morphology of rapeseed pollen particles not only has regular geometric shapes and high packing density, but also the heteroatoms (N, O, S) they carry can form numerous active sites, increase interlayer space and improve electrical conductivity to improve the performance of hard carbon. Summary of the invention

[0004] The purpose of the present invention is to overcome the problems of low first coulombic efficiency and low conductivity when hard carbon is used as the negative electrode of lithium ion batteries in the prior art, and to provide a method for preparing a biomass hard carbon lithium ion battery negative electrode material.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] A method for preparing a biomass hard carbon lithium-ion battery negative electrode material, wherein the hard carbon negative electrode material is prepared by hydrothermal reaction and high-temperature carbonization, and the hard carbon negative electrode material preparation method comprises the following steps:

[0007] S1. The harvested biomass raw material is pretreated, the pretreatment comprising: soaking the biomass raw material in a mixed solution of deionized water and ethanol, filtering and repeatedly washing with deionized water for 3 times, and drying in a vacuum drying oven after washing and filtering to obtain a pretreated material;

[0008] S2. The pretreated material is placed in a solution containing a modifier, and then stirred and dispersed, and moved into a stainless steel reactor for reaction. After the reaction is completed, the modified material is obtained by centrifugal washing, filtration and drying;

[0009] S3. The modified material is transferred to a tubular furnace and a protective gas is introduced for high-temperature carbonization to obtain a biomass hard carbon material;

[0010] The biomass raw materials include: one or more of the following: Brassica rapa, Brassica juncea and Brassica oleracea.

[0011] Furthermore, the modifier includes one or more of phosphoric acid, phosphorous acid, hydrofluoric acid, boric acid, and phytic acid.

[0012] Furthermore, the mass ratio of the pretreatment material to the modifier is 100:5-30 (20:1~10:3).

[0013] Furthermore, the reaction temperature in the reactor is 130-170° C., and the drying time is 5-24 hours.

[0014] Furthermore, the high temperature carbonization heating rate is 1-5°C / min, the maximum temperature is 1200-1500°C, and the carbonization time is 1-3h.

[0015] The beneficial effects of the present invention are:

[0016] (1) The nitrogen, oxygen, and sulfur atoms carried by the biomass raw materials themselves can form numerous active sites, increase the interlayer space, and improve the electrical conductivity to improve the electrochemical performance of hard carbon. In addition, the introduction of additional heteroatoms can further expand the interlayer spacing and repair some defects in the carbon layer, which is beneficial to improving the first coulombic efficiency of hard carbon materials.

[0017] (2) The hydrothermal treatment method used maintains the original morphology of rapeseed pollen. The elliptical particles not only help to improve the stacking density of the material, but also give the carbon material improved capacity and initial efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 A schematic diagram of a method for preparing a negative electrode material for a biomass hard carbon lithium-ion battery;

[0019] Figure 2 This is the SEM image of the biomass hard carbon negative electrode material prepared in Example 2;

[0020] Figure 3 TEM image of the biomass hard carbon negative electrode material prepared in Example 2;

[0021] Figure 4 The XPS graphs of the biomass hard carbon negative electrode materials prepared in Example 2 and Comparative Example 1;

[0022] Figure 5 XRD diagrams of biomass hard carbon negative electrode materials prepared in Examples 1-3 and Comparative Example 1;

[0023] Figure 6 This is the nitrogen isothermal adsorption curve of the biomass hard carbon lithium-ion battery negative electrode material prepared in Example 2. DETAILED DESCRIPTION

[0024] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0025] Example 1

[0026] A method for preparing a negative electrode material of a biomass hard carbon lithium-ion battery has the following steps:

[0027] (1) First, 25 g of Brassica rapa pollen was soaked in 100 mL of a mixed solution of deionized water / ethanol (v:v=7:3) for 30 min. After filtering, the upper particles were washed repeatedly with deionized water for 3 times. The pollen after the last washing was placed in a vacuum drying oven at 100°C for 12 h with a vacuum degree of -0.1 MPa.

[0028] (2) Take 5g of boric acid and dissolve it in 100mL of deionized water. Set the magnetic stirring speed to 600r / min. During the dispersion process, add 20g of the pretreated material dried in step (1). Mix for 30min. Transfer the mixed solution to a stainless steel reactor lined with polytetrafluoroethylene and place it in a forced air drying oven. Raise the temperature to 170°C at 2°C / min. The reaction time is 24h. After the reaction, first obtain rape pollen particles by centrifugation at a speed of 12000r / min. Then wash them with deionized water for 3 times. Finally, place them in a vacuum drying oven at 100°C and dry them for 12h.

[0029] (3) The modified material obtained in step (2) is loaded into a crucible and placed in a tubular furnace. Under an argon atmosphere, the temperature is first increased to 400°C at 5°C / min and kept constant for 1 hour, then increased to 1200°C at 3°C / min and kept constant for 3 hours, and then naturally cooled to room temperature to obtain a boron-doped biomass hard carbon negative electrode material, denoted as B-RP.

[0030] Example 2

[0031] A method for preparing a negative electrode material of a biomass hard carbon lithium-ion battery has the following steps:

[0032] (1) First, 25 g of Brassica rapa pollen was soaked in 100 mL of a mixed solution of deionized water / ethanol (v:v=7:3) for 30 min. After filtering, the upper particles were washed repeatedly with deionized water for 3 times. The pollen after the last washing was placed in a vacuum drying oven at 100°C for 12 h with a vacuum degree of -0.1 MPa.

[0033] (2) 3 g of phytic acid was dissolved in 100 mL of deionized water, and the magnetic stirring speed was set to 600 r / min. During the dispersion process, 20 g of the pretreated material dried in step (1) was added, and the mixing time was 30 min. The mixed solution was transferred to a stainless steel reactor lined with a polytetrafluoroethylene liner and placed in a forced air drying oven, and the temperature was raised to 150° C. at 2° C. / min. The reaction time was 24 h. After the reaction was completed, rapeseed pollen particles were first obtained by centrifugation at a speed of 11,000 r / min, and then washed with deionized water three times, and finally placed in a vacuum drying oven at 100° C. for 12 h.

[0034] (3) See Figure 2-Figure 3 The modified material obtained in step (2) is placed in a crucible and placed in a tube furnace. The temperature is first raised to 300°C at 3°C / min under an argon atmosphere, and the temperature is kept constant for 1 hour. The temperature is then raised to 1300°C at 5°C / min, and the temperature is kept constant for 3 hours. The material is then naturally cooled to room temperature to obtain a boron-doped biomass hard carbon negative electrode material, such as Figure 2 Figure 3 Shown are SEM and TEM images of the material under a microscope. The hard carbon negative electrode material of this embodiment (Example 2) is denoted as P-RP.

[0035] Example 3

[0036] A method for preparing a negative electrode material of a biomass hard carbon lithium-ion battery has the following steps:

[0037] (1) First, 25 g of Brassica rapa pollen was soaked in 100 mL of a mixed solution of deionized water / ethanol (v:v=7:3) for 30 min. After filtering, the upper particles were washed repeatedly with deionized water for 3 times. The pollen after the last washing was placed in a vacuum drying oven at 100°C for 12 h with a vacuum degree of -0.1 MPa.

[0038] (2) Take 10g of hydrogen fluoride aqueous solution (40wt.%) and disperse it in 100mL of deionized water. The magnetic stirring speed is set to 600r / min. During the dispersion process, 20g of the pretreated material dried in step (1) is added. The mixing time is 30min. The mixed solution is transferred to a stainless steel reactor lined with a polytetrafluoroethylene liner and placed in a forced air drying oven. The temperature is raised to 170°C at 2°C / min. The reaction time is 16h. After the reaction is completed, rape pollen particles are first obtained by centrifugation at a speed of 11000r / min, and then washed with deionized water for 3 times. Finally, they are placed in a vacuum drying oven at 100°C and dried for 12h.

[0039] (3) The modified material obtained in step (2) is loaded into a crucible and placed in a tubular furnace. Under an argon atmosphere, the temperature is first increased to 400°C at 5°C / min and kept constant for 1 hour, then increased to 1400°C at 3°C / min and kept constant for 3 hours, and then naturally cooled to room temperature to obtain a boron-doped biomass hard carbon negative electrode material, recorded as F-RP.

[0040] Example 4

[0041] A method for preparing a negative electrode material of a biomass hard carbon lithium-ion battery has the following steps:

[0042] (1) First, 25 g of Brassica rapa pollen was soaked in 100 mL of a mixed solution of deionized water / ethanol (v:v=7:3) for 30 min. After filtering, the upper particles were washed repeatedly with deionized water for 3 times. The pollen after the last washing was placed in a vacuum drying oven at 100°C for 12 h with a vacuum degree of -0.1 MPa.

[0043] (2) 2 g of boric acid and 2 g of phytic acid were dissolved in 100 mL of deionized water, and the magnetic stirring speed was set to 600 r / min. During the dispersion process, 20 g of the pretreated material dried in step (1) was added, and the mixing time was 30 min. The mixed solution was transferred to a stainless steel reactor lined with a polytetrafluoroethylene liner and placed in a forced air drying oven, and the temperature was raised to 160° C. at 2° C. / min. The reaction time was 24 h. After the reaction was completed, rapeseed pollen particles were first obtained by centrifugation at a speed of 12000 r / min, and then washed with deionized water for 3 times, and finally placed in a vacuum drying oven at 100° C. for 12 h.

[0044] (3) The modified material obtained in step (2) is loaded into a crucible and placed in a tubular furnace. Under an argon atmosphere, the temperature is first increased to 400°C at 5°C / min and kept constant for 1 hour, then increased to 1300°C at 3°C / min and kept constant for 3 hours, and then naturally cooled to room temperature to obtain a boron-doped biomass hard carbon negative electrode material, recorded as BP-RP.

[0045] Example 5

[0046] A method for preparing a negative electrode material of a biomass hard carbon lithium-ion battery has the following steps:

[0047] (1) First, 25 g of Brassica rapa pollen was soaked in 100 mL of a mixed solution of deionized water / ethanol (v:v=7:3) for 30 min. After filtering, the upper particles were washed repeatedly with deionized water for 3 times. The pollen after the last washing was placed in a vacuum drying oven at 100°C for 12 h with a vacuum degree of -0.1 MPa.

[0048] (2) 2 g of phytic acid and 5 g of hydrogen fluoride aqueous solution (40 wt.%) were dispersed in 100 mL of deionized water, and the magnetic stirring speed was set to 600 r / min. During the dispersion process, 20 g of the pretreated material dried in step (1) was added, and the mixing time was 30 min. The mixed solution was transferred to a stainless steel reactor lined with a polytetrafluoroethylene liner and placed in a forced air drying oven, and the temperature was raised to 150° C. at 3° C. / min. The reaction time was 24 h. After the reaction was completed, rape pollen particles were first obtained by centrifugation at a speed of 12000 r / min, and then washed with deionized water 3 times, and finally placed in a vacuum drying oven at 100° C. for 12 h.

[0049] (3) The modified material obtained in step (2) is loaded into a crucible and placed in a tubular furnace. Under an argon atmosphere, the temperature is first increased to 500°C at 5°C / min and kept constant for 1 hour, then increased to 1400°C at 3°C / min and kept constant for 3 hours, and then naturally cooled to room temperature to obtain a boron-doped biomass hard carbon negative electrode material, recorded as FP-RP.

[0050] Comparative Example 1

[0051] This comparative example is a method for preparing a biomass hard carbon negative electrode material, and the steps are as follows:

[0052] (1) First, 25 g of Brassica rapa pollen was soaked in 100 mL of a mixed solution of deionized water / ethanol (v:v=7:3) for 30 min. After filtering, the upper particles were washed repeatedly with deionized water for 3 times. The pollen after the last washing was placed in a vacuum drying oven at 100°C for 12 h with a vacuum degree of -0.1 MPa.

[0053] (2) The modified material obtained in step (1) is loaded into a crucible and placed in a tubular furnace. Under an argon atmosphere, the temperature is first increased to 500°C at 5°C / min and kept constant for 1 hour, then increased to 1300°C at 3°C / min and kept constant for 3 hours, and then naturally cooled to room temperature to obtain a boron-doped biomass hard carbon negative electrode material, denoted as RP.

[0054] The hard carbon negative electrode materials, acetylene black and polyvinylidene fluoride (PVDF) prepared in Examples 1-5 and Comparative Example 1 were mixed at a mass ratio of 8:1:1 and an appropriate amount of N-methylpyrrolidone (NMP) was added to mix evenly. The mixed slurry was then coated on a copper foil and dried at 80°C under vacuum for 12 hours. The button battery (CR2032) was prepared in an argon (H 2 O<0.1ppm,O 2 <0.1ppm) in a glove box, the counter electrode is a lithium sheet, and the electrolyte is 1M LiPF 6 In a mixture of ethylene carbonate (EC) / dimethyl carbonate (DMC) with a volume ratio of 1:1, glass fiber was used as a separator, and the charge and discharge tests were carried out on a blue power test system with a voltage range of 0.01-3.0V.

[0055] See also Figure 4-Figure 6 , respectively, compared with Example 1-Example 3, respectively:

[0056] Comparison of the binding energy strength and strength relationship of the biomass hard carbon negative electrode materials prepared in Example 2 and Comparative Example 1 (under XPS test);

[0057] XRD comparison of biomass hard carbon negative electrode materials prepared in Examples 1-3 and Comparative Example 1;

[0058] Nitrogen isotherm adsorption curve data of biomass hard carbon negative electrode material prepared in Example 2;

[0059] The test results of Examples 1-5 and Comparative Example 1 are shown in Table 1.

[0060] Table 1

[0061]

[0062] Refer to the experimental results in Table 1. Although the specific capacity of the biomass hard carbon anode material modified by heteroatom doping has increased, the reversible specific capacity of the material has been improved. This is because the introduction of heteroatoms increases the defects of the carbon material, which enhances the adsorption of lithium ions. At the same time, the defects will lead to a decrease in the first coulomb efficiency, but doping with phosphorus atoms can have a certain repair effect on the defects of the carbon material. In addition, rapeseed pollen-based biomass hard carbon anode materials can have a high specific capacity while maintaining a high first efficiency, and have good application prospects.

[0063] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.

Claims

1. A method for preparing a biomass hard carbon lithium-ion battery negative electrode material, wherein the hard carbon negative electrode material is derived from biomass and is prepared by hydrothermal reaction and high-temperature carbonization, characterized in that: The method for preparing the hard carbon negative electrode material comprises the following steps: S1. The harvested biomass raw material is pretreated, the pretreatment comprising: soaking the biomass raw material in a mixed solution of deionized water and ethanol, filtering and repeatedly washing with deionized water for 3 times, and drying in a vacuum drying oven after washing and filtering to obtain a pretreated material; S2. The pretreated material is placed in a solution containing a modifier, and then stirred and dispersed, and moved into a stainless steel reactor for reaction. After the reaction is completed, the modified material is obtained by centrifugal washing, filtration and drying; S3. The modified material is transferred to a tubular furnace and a protective gas is introduced for high-temperature carbonization to obtain a biomass hard carbon material; The biomass raw materials include: one or more of the following: Brassica rapa, Brassica juncea and Brassica oleracea.

2. The method for preparing a negative electrode material of a biomass hard carbon lithium-ion battery according to claim 1, characterized in that: The modifier includes one or more of phosphoric acid, phosphorous acid, hydrofluoric acid, boric acid, and phytic acid.

3. The method for preparing a negative electrode material of a biomass hard carbon lithium-ion battery according to claim 1, characterized in that: The mass ratio of the pretreatment material to the modifier is 100:5-30.

4. The method for preparing a negative electrode material of a biomass hard carbon lithium-ion battery according to claim 1, characterized in that: The reaction temperature in the reactor is 130-170° C., and the drying time is 5-24 hours.

5. The method for preparing a negative electrode material of a biomass hard carbon lithium-ion battery according to claim 1, characterized in that: The high temperature carbonization heating rate is 1-5℃ / min, the maximum temperature is 1200-1500℃, and the carbonization time is 1-3h.