Artificial graphite negative electrode material and preparation method thereof, negative electrode plate and battery
Through high-temperature pretreatment and water-based binder ball milling, negative electrode materials with high capacity, first-effect and high-temperature performance were prepared, which solved the problem of difficulty in taking into account both fast charging and high-temperature storage performance in the prior art, and achieved high efficiency Improved battery performance.
Patent Information
- Application Number
- CN202411154217.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The existing artificial graphite negative electrode materials are difficult to take into account both the fast charging capability and the high-temperature storage performance, and the large amount of binder used in conventional granulation methods leads to deterioration of the battery's high-temperature performance.
Through the steps of high-temperature pretreatment, crushing and shaping, water-based binder ball milling, drying and graphitization, negative electrode materials with high capacity, first-effect and high-temperature properties are prepared, reducing the amount of binder and controlling particle size and adhesiveness. The molecular weight of the catalyst is formed to form a pore structure to improve material adaptability.
It significantly improves the capacity, first effect and high temperature performance of the negative electrode material, reduces the amount of binder, enhances the material's adaptability and battery life, and reduces the preparation cost.
Smart Images

Figure CN119018887A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to an artificial graphite negative electrode material and a preparation method thereof, a negative electrode sheet and a battery. Background Art
[0002] With the development of technology, the current market has higher and higher requirements for battery technology, especially the fast charging capability and high temperature storage performance of batteries. However, the improvement of fast charging capability and the improvement of high temperature storage performance are usually opposite design directions in batteries, so it is difficult to achieve both the improvement of fast charging capability and high temperature storage performance.
[0003] The design of the negative electrode material largely determines the fast charging capability and high-temperature storage performance of the battery. Currently, the most widely used negative electrode material is artificial graphite. Artificial graphite is usually prepared by granulation to prepare secondary particles to achieve the purpose of improving fast charging capability and reducing pole piece rebound. However, in the granulation process, it is usually necessary to add a granulation binder (such as asphalt) to bond the primary particles. These binders have a lower degree of graphitization than graphite during carbonization or graphitization, high surface defects, and are easy to react with the electrolyte, resulting in deterioration of the high-temperature performance of the battery.
[0004] When the amount of binder used during granulation is high, the material has better fast charging capability and lower pole piece rebound rate, but the high temperature storage performance deteriorates significantly; when the amount of binder used during granulation is low, the high temperature storage performance of the material does not deteriorate much, but the fast charging capability and pole piece rebound rate of the material also do not change much. Therefore, there is an urgent need for an artificial graphite negative electrode material that can achieve the bonding of more primary particles at a lower binder addition amount, and achieve improved high temperature performance while ensuring the fast charging capability and rebound rate of the material.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides an artificial graphite negative electrode material and a preparation method thereof, a negative electrode sheet and a battery. The preparation process of the artificial graphite negative electrode material provided by the present invention significantly improves the gram capacity, first efficiency and high temperature performance of the negative electrode material compared with the conventional granulation method.
[0007] The present invention solves the above technical problems through the following technical solutions:
[0008] A first aspect of the present invention provides a method for preparing a negative electrode material, which comprises the following steps:
[0009] S1, roughly crushing the raw coke and performing high temperature pretreatment on the roughly crushed raw coke;
[0010] S2, crushing and shaping the raw coke pretreated in step S1 to obtain primary particles A;
[0011] S3, mixing and ball-milling the primary particles A obtained in step S2 with an aqueous binder to obtain material B;
[0012] S4, drying the material B obtained in step S3 to obtain a secondary particle precursor C;
[0013] S5, graphitizing the secondary particle precursor C obtained in step S4 to obtain a secondary particle product, namely the negative electrode material.
[0014] Preferably, in step S1, the raw coke is selected from one or more of needle coke, petroleum coke and pitch coke;
[0015] Further preferably, in step S1, the raw coke is petroleum coke.
[0016] Preferably, in step S1, the temperature of the high temperature pretreatment is 1200°C to 2000°C;
[0017] Further preferably, in step S1, the temperature of the high temperature pretreatment is 1400°C to 1800°C.
[0018] Preferably, in step S1, the high temperature pretreatment time is 1 to 10 hours;
[0019] Further preferably, in step S1, the high temperature pretreatment time is 4 to 6 hours.
[0020] Preferably, in step S2, the crushing and shaping process is performed using a roller mill and shaping machine.
[0021] Preferably, in step S2, the average particle size D50 of the primary particles A is 5 to 10 μm.
[0022] Preferably, in step S3, the mass ratio of the primary particles A to the aqueous binder is 100:(0.1-5.0);
[0023] Further preferably, in step S3, the mass ratio of the primary particles A to the aqueous binder is 100:(0.5-2.5);
[0024] Further preferably, in step S3, the mass ratio of the primary particles A to the aqueous binder is 100:(1.0-2.0).
[0025] Preferably, in step S3, the ball milling is performed by a ball mill.
[0026] Preferably, in step S3, the rotation speed of the ball mill is 50-200 r / min.
[0027] Preferably, in step S3, the ball milling temperature is room temperature.
[0028] Preferably, in step S3, the ball milling time is 3 to 5 hours.
[0029] Preferably, in step S3, the aqueous binder is selected from a binder containing one or more of carboxyl, hydroxyl, sulfonic acid, phosphoric acid, amino, carboxylate and the like groups;
[0030] Further preferably, in step S3, the aqueous binder is selected from polypropylene binders;
[0031] Further preferably, in step S3, the aqueous binder is selected from polyacrylic acid.
[0032] Preferably, in step S3, the molecular weight of the aqueous binder is in the range of 10,000 to 100,000.
[0033] Preferably, in step S4, the temperature of the drying process is 60 to 140°C;
[0034] More preferably, in step S4, the drying process is carried out at a temperature of 80-120°C.
[0035] Preferably, in step S4, the drying time is 2 to 6 hours;
[0036] More preferably, in step S4, the drying time is 3 to 5 hours.
[0037] Preferably, in step S5, the temperature of the graphitization treatment is 2500-3500°C;
[0038] More preferably, in step S5, the temperature of the graphitization treatment is 2800-3300°C.
[0039] Preferably, in step S5, the graphitization treatment time is 12 to 36 hours;
[0040] Further preferably, in step S5, the graphitization treatment time is 15 to 25 hours.
[0041] The second aspect of the present invention provides a negative electrode material, which is prepared according to the preparation method provided by the first aspect of the present invention.
[0042] A third aspect of the present invention provides a negative electrode plate, which includes the negative electrode material provided by the second aspect of the present invention.
[0043] A fourth aspect of the present invention provides a battery, comprising the negative electrode plate provided by the third aspect of the present invention.
[0044] The preparation method of the artificial graphite negative electrode material provided by the present invention significantly improves the gram capacity, first efficiency and high temperature performance of the negative electrode material compared with the conventional granulation method;
[0045] The preparation method of the present invention adds an aqueous binder so that the primary particles are bonded with the binder only at the surface functional group position to form secondary particles, thereby minimizing the amount of the binder and ensuring that the granulated material has good high-temperature performance; and the primary particles have pores, thereby alleviating volume expansion and enhancing the adaptability of the material;
[0046] The preparation method of the present invention can ensure the bonding performance of the binder to the particles by controlling the molecular weight of the aqueous binder to be in the range of 10,000 to 100,000, and can also prevent the binder from having excessive viscosity and poor fluidity, thereby causing the binder to cover the functional groups on the surface of the primary particles unevenly.
[0047] The preparation method of the present invention controls the value range of the particle size volume distribution D50 of the primary particles to be 5 to 10 μm, thereby ensuring a strong fast charging ability of the material on the basis of improving the yield of the primary particles and reducing the material cost.
[0048] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0050] Figure 1 This is a schematic diagram of the structure of the artificial graphite negative electrode material prepared in an embodiment of the present invention. DETAILED DESCRIPTION
[0051] In order to make the technical scheme and beneficial effects of the present invention more obvious and easy to understand, the following is a detailed description by listing specific embodiments. Wherein, the drawings are not necessarily drawn to scale, and local features can be enlarged or reduced to more clearly show the details of local features. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually based on conventional experimental conditions. Reagents and raw materials used in the present invention are commercially available unless otherwise specified.
[0052] In the following description, a large number of specific details are given to provide a more thorough understanding of the present application. However, it is obvious to those skilled in the art that the present application can be implemented without one or more of these details. In other examples, in order to avoid confusion with the present application, some technical features known in the art are not described; that is, all features of the actual embodiments are not described here, and well-known functions and steps are not described in detail.
[0053] The purpose of the terms used herein is only to describe specific embodiments and is not intended to be limiting of the present application. When used herein, the singular forms "one", "an" and "said / the" are also intended to include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "consisting of" and / or "comprising", when used in this specification, determine the presence of the features, integers, steps, operations, elements and / or parts, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, parts and / or groups. When used herein, the term "and / or" includes any and all combinations of the relevant listed items.
[0054] In order to thoroughly understand the present application, detailed steps and detailed structures will be presented in the following description to illustrate the technical solution of the present application. The preferred embodiments of the present application are described in detail below, but in addition to these detailed descriptions, the present application may also have other implementation methods.
[0055] Unless otherwise defined, technical and scientific terms used in this application have the same meanings as those in the technical field to which this application belongs.
[0056] If no specific techniques or conditions are specified in the following examples, the conventional techniques or conditions described in the literature in the art, or the conditions recommended by the product instructions and the manufacturer are generally used. The numerical ranges in the following examples all include the endpoint values.
[0057] A first aspect of the present invention provides a method for preparing a negative electrode material, which comprises the following steps:
[0058] S1, roughly crushing the raw coke and performing high temperature pretreatment on the roughly crushed raw coke;
[0059] S2, crushing and shaping the raw coke pretreated in step S1 to obtain primary particles A;
[0060] S3, mixing and ball-milling the primary particles A obtained in step S2 with an aqueous binder to obtain material B;
[0061] S4, drying the material B obtained in step S3 to obtain a secondary particle precursor C;
[0062] S5, graphitizing the secondary particle precursor C obtained in step S4 to obtain a secondary particle product, namely the negative electrode material.
[0063] In certain embodiments, in step S1, the raw coke is selected from one or more of needle coke, petroleum coke, and asphalt coke.
[0064] In certain embodiments, in step S1, the raw coke is petroleum coke.
[0065] In certain embodiments, in step S1, the temperature of the high temperature pretreatment is 1200°C to 2000°C.
[0066] In certain embodiments, in step S1, the temperature of the high temperature pretreatment is 1400°C to 1800°C, for example, it can be 1400°C, 1450°C, 1500°C, 1550°C, 1600°C, 1650°C, 1700°C, 1750°C or 1800°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0067] In certain embodiments, in step S1, the high temperature pretreatment time is 1 to 10 hours.
[0068] In certain embodiments, in step S1, the high temperature pretreatment time is 4 to 6 hours, for example, 4 hours, 4.5 hours, 5 hours, 5.5 hours or 6 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0069] In the embodiment of the present application, the primary particles A and the aqueous binder are bonded only at the surface functional group positions to form secondary particles, and the positions on the particle surfaces that do not contain functional groups will not be coated by the binder, thereby reducing the amount of binder used during granulation. The surface reactivity of the binder is higher than that of the primary particles A. Therefore, this method can reduce the overall reactivity of the material after granulation, that is, improve the high temperature performance of the negative electrode material and the battery; and pores are formed at the positions between the primary particles that are not coated with the binder, which has the effect of alleviating volume expansion, enhancing the adaptability of the material and improving the service life of the battery.
[0070] In certain embodiments, in step S2, the crushing and shaping process is performed using a roller mill shaping machine.
[0071] In some embodiments, in step S2, the average particle size D50 of the primary particles A is 5 to 10 μm, for example, 5.0 μm, 5.1 μm, 5.2 μm, 5.3 μm, 5.4 μm, 5.5 μm, 5.6 μm, 5.7 μm, 5.8 μm, 5.9 μm, 6.0 μm, 6.1 μm, 6.2 μm, 6.3 μm, 6.4 μm, 6.5 μm, 6.6 μm, 6.7 μm, 6.8 μm, 6.9 μm, 7.0 μm, 7.1 μm, 7.2 μm, 7.3 μm, 7.4 μm, 7.5 μm, 7.6 μm, 7.7 μm, 7.8 μm, 7.9 μm, 8.0 μm, 8.1 μm, 8.2 μm, 8.3 μm, 8.4 μm, 8.5 μm, 8.6 μm, 8.7 μm, 8.8 μm, 8.9 μm, 9.0 μm, 9.1 μm, 9.2 μm, 9.3 μm, 9.4 μm, 9.5 μm, 9.6 μm, 9.7 μm, 9.8 μm, 9.9 μm, 10.1 μm, 10.2 μm, 10.3 μm, 10.4 μm, 10.5 μm, 10.6 μm, 10.7 μm, 10.8 μm, 10.9 μm 4μm, 7.5μm, 7.6μm, 7.7μm, 7.8μm, 7.9μm, 8.0μm, 8.1μm, 8.2μm, 8.3μm, 8.4μm, 8.5μm, 8.6μm, 8.7μm, 8.8μm, 8.9μm, 9.0μm, 9.1μm, 9.2μm, 9.3μm, 9.4μm, 9.5μm, 9.6μm, 9.7μm, 9.8μm, 9.9μm or 10.0μm, but not limited to the listed values, other unlisted values within the numerical range are also applicable. Therefore, the primary particle A can have a good specific surface area and activity, reducing the agglomeration or loss of particles during the implementation process due to too small a particle size, reducing the cost of preparing negative electrode materials, and facilitating production; it also alleviates the problem of extending the transmission path of lithium ions in the material due to too large a particle size, thereby reducing the overall performance of the battery, which is beneficial to ensuring the fast charging capability of the battery.
[0072] In certain embodiments, in step S3, the mass ratio of the primary particles A to the aqueous binder is 100:(0.1-5.0).
[0073] In certain embodiments, in step S3, the mass ratio of the primary particles A to the aqueous binder is 100:(0.5-2.5).
[0074] In certain embodiments, in step S3, the mass ratio of the primary particles A and the aqueous binder is 100:(1.0-2.0), for example, it can be 100:1.0, 100:1.1, 100:1.2, 100:1.3, 100:1.4, 100:1.5, 100:1.6, 100:1.7, 100:1.8, 100:1.9 or 100:2.0, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0075] In certain embodiments, in step S3, the ball milling is performed by a ball mill.
[0076] In certain embodiments, in step S3, the rotation speed of the ball mill is 50 to 200 r / min, for example, 50 r / min, 100 r / min, 150 r / min or 200 r / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0077] In certain embodiments, in step S3, the ball milling temperature is room temperature.
[0078] In the implementation mode of the present application, the "room temperature" and "normal temperature" can be used interchangeably. They are not specific temperature values, but refer to a temperature range of 10-30°C, such as 24°C, 25°C or 26°C, but are not limited to the listed values. Other unlisted values within the numerical range are also applicable.
[0079] In certain embodiments, in step S3, the ball milling time is 3 to 5 hours, such as 3 hours, 3.5 hours, 4 hours, 4.5 hours or 5 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0080] In certain embodiments, in step S3, the aqueous binder is selected from a binder containing one or more of carboxyl, hydroxyl, sulfonic acid, phosphoric acid, amino, carboxylate and the like groups.
[0081] In certain embodiments, in step S3, the aqueous binder is selected from polypropylene binders;
[0082] In certain embodiments, in step S3, the aqueous binder is selected from polyacrylic acid.
[0083] In the embodiment of the present application, by adding an aqueous binder, the primary particles are bonded with the aqueous binder only at the surface functional group positions to form secondary particles, and the positions on the surface of the primary particles that do not contain functional groups will not be coated by the binder, thereby reducing the amount of binder used and further improving the high-temperature performance of the negative electrode material; and providing pores between the primary particles, thereby alleviating volume expansion, enhancing the adaptability of the material and improving the service life and electrochemical performance of the battery.
[0084] In some embodiments, in step S3, the molecular weight range of the aqueous binder is 10,000 to 100,000, for example, 10,000, 15,000, 20,000, 25,000, 30,000, 35,000, 40,000, 45,000, 50,000, 55,000, 60,000, 65,000, 70,000, 75,000, 80,000, 85,000, 90,000, 95,000 or 100,000, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable. As a result, the problems of poor bonding performance, insufficient bonding strength and inability to form a stable bonding interface caused by the molecular weight of the aqueous binder being lower than 10,000 are solved, so that the primary particles are tightly connected and can maintain stable shape and performance under the action of external force, thereby improving the durability of the resulting negative electrode material and extending the service life of the battery; and the problems of poor fluidity and strong viscosity caused by the molecular weight of the aqueous binder exceeding 100,000 are avoided, so that the binder can be evenly spread and penetrate into the tiny gaps between the particles, which is beneficial to the uniform coating of the functional groups on the surface of the primary particles by the aqueous binder, thereby enhancing the adaptability of the material and the service life and electrochemical performance of the battery.
[0085] In some embodiments, in step S4, the drying temperature is 60-140°C.
[0086] In some embodiments, in step S4, the temperature of the drying treatment is 80-120°C, such as 80°C, 90°C, 100°C, 110°C or 120°C, but is not limited to the listed values, and other values not listed in the numerical range are also applicable. Thus, the problem of decreased particle cohesion and low inter-particle cohesion strength caused by softening of the binder due to excessively high drying temperature is effectively prevented, and the stability of the overall structure of the negative electrode material and the service life of the battery are ensured; and the problem of the drying efficiency being greatly reduced due to the evaporation rate of water being affected by the drying temperature being too low is effectively avoided, saving energy consumption and the production cost of the material.
[0087] In certain embodiments, in step S4, the heating rate of the drying treatment is 2°C / min to 7°C / min, for example, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min or 7°C / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0088] In certain embodiments, in step S4, the drying time is 2 to 6 hours.
[0089] In certain embodiments, in step S4, the drying time is 3 to 5 hours, for example, 3 hours, 3.5 hours, 4 hours, 4.5 hours or 5 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0090] In some embodiments, in step S5, the temperature of the graphitization treatment is 2500-3500°C.
[0091] In certain embodiments, in step S5, the temperature of the graphitization treatment is 2800-3300°C, for example, 2800°C, 2900°C, 3000°C, 3100°C, 3200°C or 3300°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0092] In certain embodiments, in step S5, the graphitization treatment time is 12 to 36 hours.
[0093] In certain embodiments, in step S5, the graphitization treatment time is 15 to 25 hours, for example, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours, 24 hours or 25 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0094] A second aspect of the present invention provides a negative electrode material, which is prepared according to the preparation method described in the first aspect of the present invention.
[0095] It should be understood that, since the negative electrode material provided in the present application is prepared according to the preparation method described in the first aspect of the present invention, the beneficial effects of preparing the negative electrode material in any of the above embodiments are applicable to the negative electrode material.
[0096] A third aspect of the present invention provides a negative electrode plate, wherein the negative electrode plate comprises the negative electrode material described in the second aspect of the present invention.
[0097] It should be understood that, since the negative electrode plate provided in the present application includes the negative electrode material described in the second aspect of the present invention, the beneficial effects of preparing the negative electrode material in any of the above embodiments are applicable to the negative electrode plate.
[0098] The present application has no particular restrictions on the preparation method of the negative electrode sheet, and any preparation method known in the art may be selected as long as the purpose of the present application can be achieved.
[0099] A fourth aspect of the present invention provides a battery, comprising the negative electrode plate described in the third aspect of the present invention.
[0100] It should be understood that, since the battery provided in the present application includes the negative electrode plate described in the third aspect of the present invention, the beneficial effects of preparing the negative electrode material in any of the above embodiments are applicable to the battery.
[0101] In some embodiments, the battery may be a secondary battery, and the secondary battery may be a lithium-ion secondary battery. Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery charge and discharge process, active ions are embedded and extracted back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0102] The method of the present invention is described below by means of specific examples. It should be understood that these examples are used to illustrate the basic principles, main features and advantages of the present invention, and the present invention is not limited to the scope of the following examples; the implementation conditions adopted in the examples can be further adjusted according to specific requirements, and the implementation conditions not specified are usually the conditions in routine experiments.
[0103] Example 1
[0104] The petroleum coke was roughly broken to less than 5 mesh, and then high-temperature modified at 1500℃ for 5h. Then the primary particle A was crushed and shaped by a roller mill shaping machine, and the average particle size D50 of the primary particle A was controlled to be about 5μm, and the actual particle size D50 result was 5.3μm. Take the primary particle A and the polyacrylic acid binder according to the mass ratio of 100:2 and put them into the ball mill, and ball mill them at a speed of 100r / min at room temperature for 4h to obtain material B. Material B was placed in an oven, heated to 100℃ at a heating rate of 3℃ / min, and then kept warm for 4h, cooled and sieved to obtain the secondary particle precursor C. The secondary particle precursor C was graphitized at 3000℃ for 20h, and the secondary particle material with a particle size D50 of 9.9μm was sieved, that is, the artificial graphite negative electrode material.
[0105] Example 2
[0106] The petroleum coke was roughly broken to less than 5 mesh, and then high-temperature modified at 1500℃ for 5h. Then the primary particle A was crushed and shaped by a roller mill shaping machine, and the average particle size D50 of the primary particle A was controlled to be about 8μm, and the actual particle size D50 result was 8.3μm. Take the primary particle A and the polyacrylic acid binder according to the mass ratio of 100:1 and put them into the ball mill, and ball mill them at a speed of 100r / min at room temperature for 4h to obtain material B. Material B was placed in an oven, heated to 100℃ at a heating rate of 3℃ / min, and then kept warm for 4h, cooled and sieved to obtain the secondary particle precursor C. The secondary particle precursor C was graphitized at 3000℃ for 20h, and the secondary particle material with a particle size D50 of 12.1μm was sieved, that is, the artificial graphite negative electrode material.
[0107] Example 3
[0108] The petroleum coke was roughly broken to less than 5 mesh, and then high-temperature modified at 1500℃ for 5h. Then the primary particle A was crushed and shaped by a roller mill shaping machine, and the average particle size D50 of the primary particle A was controlled to be about 9μm, and the actual particle size D50 result was 8.1μm. Take the primary particle A and the polyacrylic acid binder according to the mass ratio of 100:1.8 and put them into the ball mill, and ball mill them at a speed of 100r / min at room temperature for 4h to obtain material B. Material B was placed in an oven, heated to 100℃ at a heating rate of 3℃ / min, and then kept warm for 4h, cooled and sieved to obtain the secondary particle precursor C. The secondary particle precursor C was graphitized at 3000℃ for 20h, and the secondary particle material with a particle size D50 of 14.6μm was sieved, that is, the artificial graphite negative electrode material.
[0109] Comparative Example 1
[0110] The petroleum coke was roughly broken to less than 5 mesh, and then high-temperature modified at 1500℃ for 5h. Then the primary particle A was crushed and shaped by a roller mill shaping machine, and the average particle size D50 of the primary particle A was controlled to be about 5μm, and the actual particle size D50 result was 5.3μm. Take the primary particle A and the petroleum asphalt with a softening point of 200℃ and an average particle size of 7μm in a mass ratio of 100:15, mix them evenly, and place them in a drum furnace. Under nitrogen protection, the temperature was raised to 750℃ at 8℃ / min and kept warm for 4h for granulation reaction, and the secondary particle precursor C was obtained by cooling and screening. The secondary particle precursor C was graphitized at 3000℃ for 20h, and the secondary particle material with a particle size D50 of 10.1μm was obtained by screening, that is, the artificial graphite negative electrode material.
[0111] Comparative Example 2
[0112] The petroleum coke was roughly broken to less than 5 mesh, and then high-temperature modified at 1500℃ for 5h. Then the primary particle A was crushed and shaped by a roller mill shaping machine, and the average particle size D50 of the primary particle A was controlled to be about 8μm, and the actual particle size D50 result was 8.3μm. Take the primary particle A and the petroleum asphalt with a softening point of 200℃ and an average particle size of 7μm in a mass ratio of 100:8 and mix them evenly. Then place them in a drum furnace, and under nitrogen protection, heat them to 750℃ at 8℃ / min and keep them warm for 4h for granulation reaction, and cool and screen to obtain the secondary particle precursor C. The secondary particle precursor C was graphitized at 3000℃ for 20h, and the secondary particle material with a particle size D50 of 11.8μm was sieved, that is, the artificial graphite negative electrode material.
[0113] Comparative Example 3
[0114] The petroleum coke was roughly broken to less than 5 mesh, and then high-temperature modified at 1500℃ for 5h. Then the primary particle A was crushed and shaped by a roller mill shaping machine, and the average particle size D50 of the primary particle A was controlled to be about 9μm, and the actual particle size D50 result was 9.1μm. The primary particle A was mixed with petroleum asphalt with a softening point of 200℃ and an average particle size of 7μm in a mass ratio of 100:13 and placed in a drum furnace. Under nitrogen protection, the temperature was raised to 750℃ at 8℃ / min and kept for 4h for granulation reaction, and the secondary particle precursor C was obtained by cooling and screening. The secondary particle precursor C was graphitized at 3000℃ for 20h, and the secondary particle material with a particle size D50 of 14.4μm was obtained by screening, that is, the artificial graphite negative electrode material.
[0115] Material performance testing
[0116] The artificial graphite negative electrode materials prepared in Examples 1-3 and Comparative Examples 1-3 were used to prepare half-cells according to the following method:
[0117] The artificial graphite negative electrode materials, SP, CMC and SBR of Examples 1-3 and Comparative Examples 1-3 were weighed respectively in a mass ratio of 95.5:1:1.5:2, stirred evenly in water to form a negative electrode slurry, and evenly coated on a copper foil. The coated electrode sheet was placed in a vacuum drying oven at a temperature of 100° C. and vacuum dried for 4 hours, and pressed into a negative electrode.
[0118] CR-2032 button cells were assembled in an argon-filled German Mikaelona glove box, using a three-component mixed solvent of 1.2 mol / L LiPF6 in a ratio of EC:DMC:EMC=1:1:1 (volume ratio) as the electrolyte and metal lithium sheets as the electrodes.
[0119] 1. Gram capacity and first coulomb efficiency (first efficiency) test: 0.05C discharge to 0.005V (recorded as C1), let stand for 5 minutes; 50μA discharge to 0.005V (recorded as C2), let stand for 5 minutes; 0.1C constant current charge to 2V (recorded as C0), let stand for 5 minutes, and end the test. Gram capacity (mAh / g) = C0 (mAh) / negative electrode material mass (g); first coulomb efficiency = C0 / (C1+C2)*100%.
[0120] 2. High temperature cycle test: Use the Xinwei charge and discharge tester, first place the battery in a 45℃ incubator and leave it for 6 hours to allow the internal temperature of the battery to reach thermal equilibrium with the incubator temperature; then charge and discharge, the charge and discharge process is: 1C constant current charge to 3.65V, then constant voltage charge to 0.05V, leave it for 10 minutes, then 1C discharge to 2.5V, leave it for 10 minutes; record the discharge capacity at this time as the first cycle discharge capacity C0, record the capacity of each cycle during the battery cycle, the capacity of the nth cycle is Cn, the capacity retention rate of the nth cycle battery = Cn / C0*100%, that is, the SOH of the battery at this time; record the number of cycles when the battery reaches 80% SOH.
[0121] The results of the gram capacity, first efficiency and high temperature cycle tests are shown in Table 1.
[0122] Table 1
[0123]
[0124] It can be concluded from Table 1 that the artificial graphite negative electrode material prepared in the embodiment of the present invention has better electrochemical performance: higher gram capacity, better first effect and better high temperature performance. Specifically, by comparing Example 1 with Comparative Example 1, Example 2 with Comparative Example 2, and Example 3 with Comparative Example 3, it can be found that compared with the corresponding comparative examples, the gram capacity and first effect of the embodiments are improved to varying degrees, and the high temperature performance is improved by 15.8% to 17.5%, while the particle size of the secondary particles produced does not change significantly and the amount of binder used is less.
[0125] It should be understood that the above embodiments are exemplary and are not intended to include all possible implementations included in the claims. Various modifications and changes may be made on the basis of the above embodiments without departing from the scope of the present disclosure. Similarly, the various technical features of the above embodiments may be arbitrarily combined to form other embodiments of the present invention that may not be explicitly described. Therefore, the above embodiments only express several implementations of the present invention and do not limit the scope of protection of the patent of the present invention.
Claims
1. A method for preparing a negative electrode material, It is characterized in that The following steps are involved: S1, roughly crushing the raw coke and performing high temperature pretreatment on the roughly crushed raw coke; S2, crushing and shaping the raw coke pretreated in step S1 to obtain primary particles A; S3, mixing and ball-milling the primary particles A obtained in step S2 with an aqueous binder to obtain material B; S4, drying the material B obtained in step S3 to obtain a secondary particle precursor C; S5, graphitizing the secondary particle precursor C obtained in step S4 to obtain a secondary particle product, namely the negative electrode material.
2. The preparation method according to claim 1, It is characterized in that In step S1, the raw coke is selected from one or more of needle coke, petroleum coke, and pitch coke, preferably petroleum coke; Preferably, the temperature of the high temperature pretreatment is 1200°C to 2000°C, preferably 1400°C to 1800°C; Preferably, the high temperature pretreatment time is 1 to 10 hours, preferably 4 to 6 hours.
3. The preparation method according to claim 1, It is characterized in that In step S2, the crushing and shaping process is performed by a roller mill shaping machine; Preferably, the average particle size D50 of the primary particles A is 5 to 10 μm.
4. The preparation method according to claim 1, It is characterized in that In step S3, the mass ratio of the primary particles A to the aqueous binder is 100:(0.1-5.0); Preferably, the mass ratio of the primary particles A to the aqueous binder is 100:(0.5-2.5); Preferably, the mass ratio of the primary particles A to the aqueous binder is 100:(1.0-2.0); Preferably, the ball milling is performed by a ball mill; Preferably, the rotation speed of the ball mill is 50 to 200 r / min; Preferably, the ball milling temperature is room temperature; Preferably, the ball milling time is 3 to 5 hours.
5. The preparation method according to claim 1 or 4, It is characterized in that In step S3, the aqueous binder is selected from a binder containing one or more of a carboxyl group, a hydroxyl group, a sulfonic acid group, a phosphoric acid group, an amino group, a carboxylate group, and the like; Preferably, the aqueous binder is selected from polypropylene binders; Preferably, the aqueous binder is selected from polyacrylic acid; Preferably, the molecular weight of the aqueous binder is in the range of 10,000 to 100,000.
6. The preparation method according to claim 1, It is characterized in that In step S4, the drying temperature is 60 to 140° C., preferably 80 to 120° C.; Preferably, the drying time is 2 to 6 hours, preferably 3 to 5 hours.
7. The preparation method according to claim 1, It is characterized in that In step S5, the temperature of the graphitization treatment is 2500-3500° C., preferably 2800-3300° C.; Preferably, the graphitization treatment time is 12 to 36 hours, preferably 15 to 25 hours.
8. A negative electrode material, It is characterized in that The negative electrode material is prepared according to the preparation method described in any one of claims 1-7.
9. A negative electrode sheet, It is characterized in that The negative electrode plate comprises the negative electrode material as claimed in claim 8.
10. A battery, It is characterized in that The battery comprises the negative electrode sheet as claimed in claim 9.
Citation Information
Patent Citations
Graphene coated graphite composite lithium ion battery negative material and its preparation method
CN104332616A
Graphitized carbon-coated electrode material, preparation method thereof and application thereof as electrode material of energy storage devices
CN108155353A
Silicon-carbon negative electrode material and preparation method thereof
CN109713265A
Preparation method of artificial graphite negative electrode material and negative electrode material
CN117059803A
Method for manufacturing negative electrode material for lithium ion secondary battery