Preparation method of gas-sensitive material and gas-sensitive material
By using hydrothermal reaction between porous graphene and tin dioxide in gas-sensitive materials, the problems of low sensitivity and complex preparation of existing gas-sensitive materials are solved, and efficient and simple preparation of gas sensing materials is achieved, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202411113609.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
The existing gas-sensitive materials have low sensitivity, long response time, complex preparation steps, low preparation efficiency, and difficult to effectively monitor harmful gases that are threatened by the environment and health.
Porous graphene/tin dioxide gas-sensitive materials were prepared by ultrasonic dispersion and hydrothermal reaction with components such as stannous chloride, citric acid and sodium hydroxide, which simplified the preparation process and Improves the sensitivity and response speed of the material.
It improves the sensitivity and response speed of gas-sensitive materials, simplifies the preparation steps, reduces the complexity of equipment and production costs, and is suitable for industrial mass production.
Smart Images

Figure CN119018932A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present disclosure relate to the field of material technology, and in particular, to a method for preparing a gas-sensitive material and the gas-sensitive material. Background Art
[0002] The combustion of fossil fuels like coal and oil, the leakage of various waste gases during industrial manufacturing, and the release of harmful gases from furniture and building materials in our daily lives not only pollute the environment but also endanger human health. Therefore, there is an urgent need to develop gas sensing technology and equipment to effectively and in real time monitor gases that threaten the environment and human health.
[0003] In the related art, a single tin dioxide gas-sensitive material is generally prepared. The single tin dioxide gas-sensitive material has poor performance, low sensitivity, long response time, complex preparation steps and low preparation efficiency. Summary of the Invention
[0004] The purpose of the present disclosure is to provide a method for preparing a gas-sensitive material and a gas-sensitive material, thereby overcoming, at least to a certain extent, the problems of complex preparation steps and low preparation efficiency of the gas-sensitive material caused by the limitations and defects of the relevant technologies.
[0005] According to one aspect of the present disclosure, a method for preparing a gas-sensitive material is provided, comprising: using porous graphene as a starting material, ultrasonically dispersing a porous graphene ethanol aqueous solution to obtain a first solution; using stannous chloride as a tin source, citric acid as a surfactant, and sodium hydroxide as a precipitant, dissolving the tin source, the surfactant, and the precipitant in the ethanol aqueous solution in sequence to obtain a suspension; adding the suspension dropwise to the first solution to obtain a mixed solution; transferring the mixed solution to a reactor for a hydrothermal reaction, and cooling to room temperature after the hydrothermal reaction for centrifugation, washing, and freeze-drying to obtain a porous graphene / tin dioxide gas-sensitive material.
[0006] In an exemplary embodiment of the present disclosure, the molar ratio of the precipitant to the tin source is a first molar ratio, and the first molar ratio is 20:1 to 5:1.
[0007] In an exemplary embodiment of the present disclosure, the molar ratio of the tin source to the surfactant is a second molar ratio, and the second molar ratio is 1:1.
[0008] In an exemplary embodiment of the present disclosure, the reaction temperature of the hydrothermal reaction is 160 to 200° C., and the reaction time of the hydrothermal reaction is 6 to 18 hours.
[0009] In an exemplary embodiment of the present disclosure, the size of the tin dioxide gas-sensitive material in the porous graphene / tin dioxide gas-sensitive material is 300-500 nm, and the tin dioxide gas-sensitive material is uniformly distributed on the surface of the porous graphene.
[0010] In an exemplary embodiment of the present disclosure, the freeze-drying time is 48 to 60 hours.
[0011] In an exemplary embodiment of the present disclosure, stannous chloride is used as a tin source, citric acid is used as a surfactant, and sodium hydroxide is used as a precipitant. The tin source, the surfactant, and the precipitant are dissolved in an ethanol aqueous solution in sequence to obtain a suspension, including: dissolving the tin source in the ethanol aqueous solution and stirring to obtain a second suspension; dissolving the surfactant in the ethanol aqueous solution, stirring and adding dropwise to the second suspension to obtain a third suspension; dissolving the precipitant in the ethanol aqueous solution, stirring and adding dropwise to the third suspension to obtain a fourth suspension, and using the fourth suspension as the suspension.
[0012] In an exemplary embodiment of the present disclosure, the method further includes: preparing the gas-sensitive material into a slurry, coating the slurry on a ceramic tube, and assembling the slurry into a gas-sensitive element; and performing a gas-sensitive performance test on the gas-sensitive element to determine the gas-sensitive response and response time.
[0013] In an exemplary embodiment of the present disclosure, the gas-sensitive performance test of the gas-sensitive element to determine the gas-sensitive response and response time includes: performing a gas-sensitive performance test on the gas-sensitive element in acetone gas at an operating temperature of 280° C. to determine the gas-sensitive response and response time.
[0014] According to one aspect of the present disclosure, a gas-sensitive material is provided. The gas-sensitive material is prepared according to any one of the above methods for preparing a gas-sensitive material.
[0015] In the technical solution provided in the embodiment of the present disclosure, on the one hand, porous graphene is used as a starting material, stannous chloride is used as a tin source, citric acid is used as a surfactant, and sodium hydroxide is used as a precipitant to prepare a suspension, the suspension is added dropwise to a first solution represented by a porous graphene dispersion to obtain a mixed solution, the mixed solution is transferred to a reactor for hydrothermal reaction, cooled to room temperature, centrifuged and washed, and freeze-dried to obtain a porous graphene / tin dioxide gas-sensitive material. Compared with single tin dioxide, graphene / tin dioxide gas-sensitive materials have improved sensitivity, reduced response time, strong selectivity, and effectively improved their gas-sensitive performance. On the other hand, porous graphene / tin dioxide gas-sensitive materials can be prepared by only a simple hydrothermal reaction, with simple operating steps and no need for complex instruments and equipment, thereby reducing preparation complexity and improving preparation efficiency.
[0016] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The accompanying drawings are incorporated into and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification, are used to explain the principles of the present disclosure. Obviously, the drawings described below are only some embodiments of the present disclosure, and those skilled in the art can derive other drawings based on these drawings without inventive effort.
[0018] Figure 1 A flow chart schematically illustrates a method for preparing a gas-sensitive material in an embodiment of the present disclosure.
[0019] Figure 2 The XRD pattern of the porous graphene / tin dioxide gas-sensitive material is schematically shown.
[0020] Figure 3 The SEM image of the porous graphene / tin dioxide gas-sensitive material prepared according to Example 1 is schematically shown.
[0021] Figure 4 The response recovery curve obtained by assembling the porous graphene / tin dioxide gas-sensitive material prepared in Example 1 into a gas-sensitive element is schematically shown.
[0022] Figure 5 The SEM image of the porous graphene / tin dioxide gas-sensitive material prepared according to Example 2 is schematically shown.
[0023] Figure 6 The response recovery curve obtained by assembling the porous graphene / tin dioxide gas-sensitive material prepared in Example 2 into a gas-sensitive element is schematically shown.
[0024] Figure 7 The SEM image of the porous graphene / tin dioxide gas-sensitive material prepared according to Example 3 is schematically shown.
[0025] Figure 8 The porous graphene / tin dioxide gas-sensitive material prepared according to Example 3 is assembled into a gas-sensitive element and tested in a line graph of gas-sensitive responses corresponding to different operating temperatures.
[0026] Figure 9 The gas-sensitive response bar chart corresponding to different gases tested by assembling the porous graphene / tin dioxide gas-sensitive material prepared according to Example 3 into a gas-sensitive element is schematically shown.
[0027] Figure 10The response recovery curve obtained by assembling the porous graphene / tin dioxide gas-sensitive material prepared according to Example 3 into a gas-sensitive element is schematically shown.
[0028] Figure 11 The SEM image of the porous graphene / tin dioxide gas-sensitive material prepared according to Example 4 is schematically shown.
[0029] Figure 12 The response recovery curve obtained by assembling the porous graphene / tin dioxide gas-sensitive material prepared according to Example 4 into a gas-sensitive element is schematically shown.
[0030] Figure 13 The SEM image of the porous graphene / tin dioxide gas-sensitive material prepared according to Example 5 is schematically shown.
[0031] Figure 14 The response recovery curve obtained by assembling the porous graphene / tin dioxide gas-sensitive material prepared according to Example 5 into a gas-sensitive element is schematically shown. DETAILED DESCRIPTION
[0032] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the examples set forth herein; rather, these embodiments are provided so that the present disclosure will be more comprehensive and complete and will fully convey the concepts of the example embodiments to those skilled in the art. The described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or that other methods, components, devices, steps, etc. may be employed. In other cases, well-known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.
[0033] The terms "a", "an", "the" and "said" are used in this specification to indicate the presence of one or more elements / components, etc.; the terms "including" and "having" are used to express open-ended inclusion and mean that additional elements / components, etc. may exist in addition to the listed elements / components, etc.; the terms "first" and "second" are used only as labels and are not intended to limit the quantity of their objects.
[0034] Tin dioxide is a typical direct bandgap n-type semiconductor with excellent semiconductor, optical, and electrical properties, and a wide bandgap (3.6 eV). Its nanomaterial preparation method is simple and has a wide range of applications in gas-sensitive materials, luminescent materials, catalyst materials, and lithium-ion battery anode materials. Currently, as a widely used semiconductor material, tin dioxide has good gas-sensing properties for reducing gases such as hydrogen, ethanol, and acetone. However, it still suffers from disadvantages such as low sensitivity, slow response recovery, high operating temperature, and poor selectivity for oxidizing gases. Numerous studies have shown that graphene / metal oxide gas-sensitive materials can effectively overcome the problems of single metal oxides in gas sensor applications. Although the low response and high operating temperature of graphene-based gas sensors have been improved, the problems of poor selectivity and slow response-recovery speed still exist.
[0035] In order to solve the above technical problems, the present disclosure provides a method for preparing a gas-sensitive material, which is used to prepare the gas-sensitive material. Figure 1 As shown in , it mainly includes the following steps:
[0036] In step S110, porous graphene is used as a starting material, and an ethanol aqueous solution of porous graphene is ultrasonically dispersed to obtain a first solution;
[0037] In step S120, stannous chloride is used as a tin source, citric acid is used as a surfactant, and sodium hydroxide is used as a precipitant. The tin source, the surfactant, and the precipitant are dissolved in an ethanol aqueous solution in sequence to obtain a suspension.
[0038] In step S130, the suspension is added dropwise to the first solution to obtain a mixed solution;
[0039] In step S140, the mixed solution is transferred to a reactor for hydrothermal reaction, and after the hydrothermal reaction, it is cooled to room temperature for centrifugation, washing, and freeze-drying to obtain a porous graphene / tin dioxide gas-sensitive material.
[0040] In the embodiment of the present disclosure, on the one hand, porous graphene is used as the starting material, stannous chloride is used as the tin source, citric acid is used as the surfactant, and sodium hydroxide is used as the precipitant to prepare a suspension, the suspension is added dropwise to the first solution to prepare a mixed solution, the mixed solution is transferred to a reactor for hydrothermal reaction, cooled to room temperature, centrifuged and washed, and freeze-dried to obtain a porous graphene / tin dioxide gas-sensitive material. Compared with single tin dioxide, the graphene / tin dioxide gas-sensitive material has a porous structure in the graphene that greatly increases the surface area of the material, provides a large number of active sites for the adsorption of the test gas, and can become an ideal transmission channel for the test gas, effectively promoting the diffusion of gas molecules through its micro / nanopores. By introducing porous graphene and metal oxide composites, the problems existing in the application of single metal oxides in gas sensors can be overcome, the sensitivity is improved, the response time is reduced, and its gas-sensitive performance is effectively improved. On the other hand, only a simple hydrothermal reaction is required to prepare the porous graphene / tin dioxide gas-sensitive material, the operation steps are simple, and no complex instruments and equipment are required, thereby reducing the preparation complexity and improving the preparation efficiency.
[0041] Next, combine Figure 1 The preparation method of the gas-sensitive material in the embodiment of the present disclosure is described in detail.
[0042] In step S110 , porous graphene is used as a starting material, and an ethanol-water solution of porous graphene is ultrasonically dispersed to obtain a first solution.
[0043] In the disclosed embodiments, porous graphene refers to a carbon material having nanoscale pores on a two-dimensional basal surface. Porous graphene can be prepared by metal etching, using porous graphene as a starting material. After obtaining the porous graphene, a 33 vol% ethanol aqueous solution can be ultrasonically dispersed to obtain a first solution, which can be designated as Solution I.
[0044] In step S120, stannous chloride is used as a tin source, citric acid is used as a surfactant, and sodium hydroxide is used as a precipitant. The tin source, the surfactant, and the precipitant are dissolved in an ethanol aqueous solution in sequence to obtain a suspension.
[0045] In the disclosed embodiments, a tin source, a surfactant, and a precipitant can be sequentially dissolved in an ethanol-water solution and rapidly stirred to obtain a final suspension. Stannous chloride can be used as the tin source, citric acid can be used as the surfactant, and sodium hydroxide can be used as the precipitant. In addition, other components can also be used as the tin source, surfactant, and precipitant, and are not specifically limited herein.
[0046] For example, a tin source can be dissolved in an ethanol-water solution and stirred to obtain a second suspension; a surfactant can be dissolved in an ethanol-water solution, stirred, and added dropwise to the second suspension to obtain a third suspension; a precipitant can be dissolved in an ethanol-water solution, stirred, and added dropwise to the third suspension to obtain a fourth suspension, with the fourth suspension serving as the suspension. The ethanol-water solutions used to dissolve the tin source, precipitant, and surfactant can be stored in different containers, and the ethanol-water solutions in the different containers can have the same composition. Specifically, stannous chloride can be used as the tin source and dissolved in a 33 vol% ethanol-water solution in a first container, rapidly stirred to obtain a second suspension, i.e., Suspension II; citric acid can be used as the surfactant and dissolved in a 33 vol% ethanol-water solution in a second container, rapidly stirred, and added dropwise to Suspension II to obtain a third suspension, i.e., Suspension III; sodium hydroxide can be used as the precipitant and dissolved in a 33 vol% ethanol-water solution in a third container, rapidly stirred, and the suspension in the third container can be added dropwise to Suspension III to obtain a fourth suspension, i.e., Suspension IV.
[0047] In step S130 , the suspension is added dropwise to the first solution to obtain a mixed solution.
[0048] In the embodiment of the present disclosure, the suspension can be added dropwise to the first solution to obtain a mixed solution. For example, the suspension IV can be added dropwise to the porous graphene dispersion, i.e., solution I, to obtain a mixed solution V.
[0049] In the process of adding the suspension dropwise to the first solution, the precipitant and the tin source can be added in different molar ratios, and the tin source and the surfactant can be added in the same molar ratio. Specifically, the molar ratio of the precipitant to the tin source is a first molar ratio, and the molar ratio of the tin source to the surfactant can be a second molar ratio, wherein the first molar ratio can be 20:1 to 5:1, and the second molar ratio can be 1:1. For example, the first molar ratio can be 5:1, 10:1, 20:1, or other ratios. Based on this, the content of the tin source, surfactant, and precipitant can be adjusted, and the content of the tin source, surfactant, and precipitant can be, for example: 1 mmol of tin source, 1 mmol of surfactant, 10 mmol of precipitant; 0.5 mmol of tin source, 0.5 mmol of surfactant, 10 mmol of precipitant; 2 mmol of tin source, 2 mmol of surfactant, 10 mmol of precipitant.
[0050] In step S140, the mixed solution is transferred to a reactor for hydrothermal reaction, and after the hydrothermal reaction, it is cooled to room temperature for centrifugation, washing, and freeze-drying to obtain a porous graphene / tin dioxide gas-sensitive material.
[0051] In the embodiment of the present disclosure, the mixed solution V can be transferred to a reactor for a hydrothermal reaction. A hydrothermal reaction is a chemical process in which water as a solvent reacts with other substances under high pressure and high temperature. The hydrothermal reaction is usually carried out in a closed reaction vessel, and the reaction temperature is usually above 100°C and the pressure is above normal pressure to increase the reaction rate and change the composition of the reaction products. In some embodiments, the reaction temperature of the hydrothermal reaction can be 160 to 200°C, and the reaction time of the hydrothermal reaction can be 6 to 18 hours, for example, 6 hours, 12 hours, 18 hours, and so on. The reaction temperature and reaction time of the hydrothermal reaction can be adjusted according to actual needs. For example, the reaction temperature of the hydrothermal reaction can be 160°C, 180°C, or 200°C.
[0052] After the hydrothermal reaction, the mixture can be cooled to room temperature and centrifuged, washed, and freeze-dried to obtain a gas-sensitive material. The gas-sensitive material can be a porous graphene / tin dioxide gas-sensitive material, that is, a tin dioxide gas-sensitive material is generated on the surface of the porous graphene. The size of the tin dioxide gas-sensitive material in the porous graphene / tin dioxide gas-sensitive material is 300 to 500 nm, and the tin dioxide gas-sensitive material is uniformly distributed on the surface of the porous graphene. The freeze-drying time can be 48 to 60 hours, for example, 48 hours, 55 hours, or 60 hours, and can also be adjusted according to actual needs.
[0053] After the gas-sensitive material is prepared, it can be added to ultrapure water to form a slurry, which can be coated on a ceramic tube to assemble it into a gas-sensitive element, so as to perform a gas-sensitive performance test through the gas-sensitive element.
[0054] Next, the preparation method of the gas-sensitive material in the embodiment of the present disclosure is described in detail.
[0055] Example 1
[0056] The preparation method of the gas-sensitive material specifically comprises the following steps:
[0057] Step 1: Prepare porous graphene using a simple metal etching method and use it as a starting material to ultrasonically disperse porous graphene in a 33% ethanol aqueous solution, which is recorded as the first solution, i.e., Solution I.
[0058] Step 2: Using stannous chloride as a tin source, weigh 1 mm² and dissolve it in a 33% ethanol aqueous solution, stirring rapidly to obtain a second suspension, i.e., suspension II.
[0059] Step 3: Using citric acid as a surfactant, weigh 1 mm², dissolve it in 33% ethanol aqueous solution, stir rapidly, and add it dropwise to the suspension II to obtain a third suspension, namely, suspension III;
[0060] Step 4: Using sodium hydroxide as a precipitant, weigh 10 mm², dissolve it in 33% ethanol aqueous solution, stir rapidly, and add it dropwise to the suspension III to obtain a fourth suspension, i.e., suspension IV;
[0061] Step 5: adding the suspension IV dropwise into the porous graphene dispersion (first solution) to obtain a mixed solution V; wherein the molar ratio of the precipitant sodium hydroxide to the tin source stannous chloride is 10:1; and the molar ratio of the tin source stannous chloride to the surfactant citric acid is 1:1;
[0062] Step 6: Transfer the mixed solution V to a reactor and perform a hydrothermal reaction at 160°C for 12 hours. The mixture is then cooled to room temperature, centrifuged, washed, and freeze-dried for 48 hours to obtain the final product, a porous graphene / tin dioxide gas-sensitive material. The gas-sensitive material is a flower-cluster-shaped gas-sensitive material.
[0063] Step 7: Add ultrapure water to the final product gas-sensitive material to form a slurry, apply it on a ceramic tube, assemble it into a gas-sensitive element, and test the gas-sensitive performance.
[0064] Figure 2 The schematic diagram of X-ray diffraction test on gas sensitive materials is shown schematically in Figure 2 As shown in the figure, the peaks at 2θ=26.6°, 33.9°, 37.9°, 38.9°, 42.6°, 51.8°, 54.7°, 57.8°, 61.9°, 64.7° and 65.9° in the spectrum correspond to the (110), (101), (200), (111), (210), (211), (220), (002) (310), (112) and (301) crystal planes of tin dioxide, among which no graphene peaks were found. This may be because the characteristic peaks of tin dioxide are too strong to cover up the peaks of graphene.
[0065] Figure 3 The schematic diagram of scanning electron microscopy of the gas-sensitive material prepared in Example 1 is shown schematically in FIG. Figure 3 As shown in the figure, a large number of non-uniform rod-like structures (about 200 nm in size) are dispersed on the surface of the porous graphene, and a small number of irregular flower-like tin dioxide (about 300 nm in size) are distributed on the surface of the porous graphene, which is similar to the nucleation stage of the grains. This may be because the hydrothermal temperature is too low, resulting in the incomplete development of the tin dioxide flower-like structure.
[0066] Next, the gas-sensitive material prepared in Example 1 was assembled into a gas-sensitive element to test its gas-sensitive performance. Figure 4 As shown in , when the operating temperature is 280°C, the gas sensitive response of the gas sensitive material to 50ppm acetone gas is 7.8, and the response time is 18s.
[0067] Example 2
[0068] Compared with Example 1, the contents of the tin source and the surfactant are reduced, and the reaction temperature of the hydrothermal reaction is increased. The preparation method of the gas-sensitive material specifically includes the following steps:
[0069] Step 1: Prepare porous graphene using a simple metal etching method and use it as a starting material to ultrasonically disperse porous graphene in a 33 vol% ethanol aqueous solution, which is recorded as the first solution, i.e., Solution I.
[0070] Step 2: Using stannous chloride as a tin source, weigh 0.5 mmol, dissolve it in a 33 vol% ethanol aqueous solution, and rapidly stir to obtain a second suspension, i.e., suspension II;
[0071] Step 3: Using citric acid as a surfactant, weigh 0.5 mmol, dissolve it in 33 vol% ethanol aqueous solution, stir rapidly, and add it dropwise to the suspension II to obtain a third suspension, i.e., suspension III;
[0072] Step 4: Using sodium hydroxide as a precipitant, weigh 10 mmol, dissolve it in 33 vol% ethanol aqueous solution, stir rapidly, and add it dropwise to the suspension III to obtain a fourth suspension, i.e., suspension IV;
[0073] Step 5: adding the suspension IV dropwise into the porous graphene dispersion (first solution) to obtain a mixed solution V; wherein the molar ratio of the precipitant sodium hydroxide to the tin source stannous chloride is 20:1; and the molar ratio of the tin source stannous chloride to the surfactant citric acid is 1:1;
[0074] Step 6: Transfer the mixed solution V to a reactor for hydrothermal reaction. The reaction temperature of the hydrothermal reaction is 180°C and the insulation time is 12 hours. After the hydrothermal reaction is completed, cool to room temperature, centrifuge, wash, and then freeze-dry for 48 hours to obtain the final product, which is a porous graphene / tin dioxide gas-sensitive material.
[0075] Step 7: Add ultrapure water to the final product gas-sensitive material to form a slurry, apply it on a ceramic tube, assemble it into a gas-sensitive element, and test the gas-sensitive performance.
[0076] Figure 2 The schematic diagram of X-ray diffraction test on gas sensitive materials is shown schematically in Figure 2 As shown in , there is an obvious diffraction peak corresponding to tin dioxide in the spectrum, but no diffraction peak of graphene is found. This may be because the characteristic peak of tin dioxide is stronger, which covers the peak of graphene.
[0077] Figure 5 The schematic diagram of the gas-sensitive material prepared in Example 2 is shown schematically in FIG. Figure 5As shown in the figure, it can be seen that flower-like tin dioxide (about 300 nm in size) is distributed on the surface of porous graphene, but the flower-like structure of tin dioxide is not uniform, and there are a small number of rod-like structures. This may be because excessive sodium hydroxide inhibits the growth of flower-like tin dioxide.
[0078] Figure 6 FIG2 schematically shows a schematic diagram of assembling the gas-sensitive material prepared in Example 2 into a gas-sensitive element for gas-sensitive performance testing. Figure 6 As shown, when the working temperature is 280℃, the gas sensitive response to 50ppm acetone gas is 8.5 and the response time is 11s.
[0079] Example 3
[0080] Compared with Example 1, the reaction temperature of the hydrothermal reaction is increased. Based on this, the preparation method of the gas-sensitive material specifically includes the following steps:
[0081] Step 1: Prepare porous graphene using a simple metal etching method and use it as a starting material to ultrasonically disperse porous graphene in a 33 vol% ethanol aqueous solution, which is recorded as the first solution, i.e., Solution I.
[0082] Step 2: Using stannous chloride as a tin source, weigh 1 mmol, dissolve it in a 33 vol% ethanol aqueous solution, and rapidly stir to obtain a second suspension, i.e., suspension II;
[0083] Step 3: Using citric acid as a surfactant, weigh 1 mmol, dissolve it in 33 vol% ethanol aqueous solution, stir rapidly, and add it dropwise to the suspension II to obtain a third suspension, i.e., suspension III;
[0084] Step 4: Using sodium hydroxide as a precipitant, weigh 10 mmol, dissolve it in 33 vol% ethanol aqueous solution, stir rapidly, and add it dropwise to the suspension III to obtain a fourth suspension, i.e., suspension IV;
[0085] Step 5: adding the suspension IV dropwise into the porous graphene dispersion (first solution) to obtain a mixed solution V; wherein the molar ratio of the precipitant sodium hydroxide to the tin source stannous chloride is 10:1; and the molar ratio of the tin source stannous chloride to the surfactant citric acid is 1:1;
[0086] Step 6: Transfer the mixed solution V to a reactor for hydrothermal reaction. The reaction temperature of the hydrothermal reaction is 180°C and the insulation time is 12 hours. After the hydrothermal reaction, cool to room temperature, centrifuge and wash, and then freeze-dry for 48 hours to obtain the final product, which is a porous graphene / tin dioxide gas-sensitive material.
[0087] Step 7: Add ultrapure water to the final product gas-sensitive material to form a slurry, apply it on a ceramic tube, assemble it into a gas-sensitive element, and test the gas-sensitive performance.
[0088] Figure 2 The schematic diagram of X-ray diffraction test on gas sensitive materials is shown schematically in Figure 2 As shown in , there is an obvious diffraction peak corresponding to tin dioxide in the spectrum, but no diffraction peak of graphene is found. This may be because the characteristic peak of tin dioxide is stronger, which covers the peak of graphene.
[0089] Figure 7 The schematic diagram of the gas-sensitive material prepared in Example 3 is shown schematically in FIG. Figure 7 As shown in , it can be seen that flower-like tin dioxide (about 500 nm in size) is evenly distributed on the surface of porous graphene, presenting a good flower cluster structure.
[0090] Figure 8 FIG2 schematically shows a schematic diagram of assembling the gas-sensitive material prepared in Example 3 into a gas-sensitive element for gas-sensitive performance testing. Figure 8 As shown in the figure, the gas sensitive response test of acetone gas is carried out in the working temperature range of 220~320℃. Figure 8 As shown, it is found that when the working temperature is 280℃, the gas sensitive response value is the highest, and the gas sensitive response value is 19.2. Therefore, the optimal working temperature of the gas sensor is 280℃.
[0091] like Figure 9 The porous graphene / zinc oxide gas-sensing material prepared in Example 3 was assembled into a gas sensor, and its gas-sensing response was tested at its optimal operating temperature for test gases. For example, the test gases could be 50 ppm of acetone, isopropanol, ethanol, and other eight gases. As can be seen from the gas-sensing response values obtained at the optimal operating temperature of 280°C, the porous graphene / zinc oxide gas-sensing material exhibited the best gas-sensing response to acetone.
[0092] At the same time, the response recovery characteristics of the porous graphene / zinc oxide gas-sensitive material were tested, such as Figure 10 As shown, the response time is only 8s, which is faster than the response time of most gas-sensitive materials such as tin dioxide used in industrial applications.
[0093] Example 4
[0094] Compared with Example 1, the contents of the tin source and the surfactant are increased, and the reaction temperature of the hydrothermal reaction is increased. The method for preparing the gas-sensitive material comprises the following steps:
[0095] Step 1: Prepare porous graphene using a simple metal etching method and use it as a starting material to ultrasonically disperse porous graphene in a 33 vol% ethanol aqueous solution, which is recorded as the first solution, i.e., Solution I.
[0096] Step 2: Using stannous chloride as a tin source, weigh 2 mmol, dissolve it in a 33 vol% ethanol aqueous solution, and rapidly stir to obtain a second suspension, i.e., suspension II;
[0097] Step 3: Using citric acid as a surfactant, weigh 2 mmol, dissolve it in 33 vol% ethanol aqueous solution, stir rapidly, and add it dropwise to the suspension II to obtain a third suspension, i.e., suspension III;
[0098] Step 4: Using sodium hydroxide as a precipitant, weigh 10 mmol, dissolve it in 33 vol% ethanol aqueous solution, stir rapidly, and add it dropwise to the suspension III to obtain a fourth suspension, i.e., suspension IV;
[0099] Step 5: adding the suspension IV dropwise to the first solution represented by the porous graphene dispersion to obtain a mixed solution V; wherein the molar ratio of the precipitant sodium hydroxide to the tin source stannous chloride is 5:1; and the molar ratio of the tin source stannous chloride to the surfactant citric acid is 1:1;
[0100] Step 6: Transfer the mixed solution V to a reactor for hydrothermal reaction. The reaction temperature of the hydrothermal reaction is 180°C and the insulation time is 12 hours. After the hydrothermal reaction, cool to room temperature, centrifuge, wash, and then freeze-dry for 48 hours to obtain the final product, i.e., a porous graphene / tin dioxide gas-sensitive material.
[0101] Step 7: Add ultrapure water to the final product gas-sensitive material to form a slurry, apply it on a ceramic tube, assemble it into a gas-sensitive element, and perform a gas-sensitive performance test.
[0102] Figure 2 The schematic diagram of X-ray diffraction test on gas sensitive materials is shown schematically in Figure 2 As shown in , there is an obvious diffraction peak corresponding to tin dioxide in the spectrum, but no diffraction peak of graphene is found. This may be because the characteristic peak of tin dioxide is stronger, which covers the peak of graphene.
[0103] Figure 11 The schematic diagram of scanning electron microscopy of the gas-sensitive material prepared in Example 4 is shown schematically in FIG. Figure 11 As shown in , it can be seen that tin dioxide is accumulated on the surface of the porous graphene in the form of irregular spheres, the size of which is significantly smaller than that in Example 3, and agglomeration occurs. Therefore, the addition of excessive stannous chloride will lead to an increase in the surface density of tin dioxide on the porous graphene, which will lead to a decrease in its gas-sensing performance.
[0104] Figure 12 FIG2 schematically shows a schematic diagram of assembling the gas-sensitive material prepared in Example 4 into a gas-sensitive element for gas-sensitive performance testing. Figure 12As shown in the figure, when the working temperature is 280℃, the gas sensitive response to 50ppm acetone gas is 11.8 and the response time is 18s.
[0105] Example 5
[0106] Compared with Example 1, the reaction temperature of the hydrothermal reaction is increased. The preparation method of the gas-sensitive material comprises the following steps:
[0107] Step 1: Prepare porous graphene using a simple metal etching method and use it as a starting material to ultrasonically disperse porous graphene in a 33 vol% ethanol aqueous solution, which is recorded as the first solution, i.e., Solution I.
[0108] Step 2: Using stannous chloride as a tin source, weigh 1 mmol, dissolve it in a 33 vol% ethanol aqueous solution, and rapidly stir to obtain a second suspension, i.e., suspension II;
[0109] Step 3: Using citric acid as a surfactant, weigh 1 mmol, dissolve it in 33 vol% ethanol aqueous solution, stir rapidly, and add it dropwise to the suspension II to obtain a third suspension, i.e., suspension III;
[0110] Step 4: Using sodium hydroxide as a precipitant, weigh 10 mmol, dissolve it in 33 vol% ethanol aqueous solution, stir rapidly, and add it dropwise to the suspension III to obtain a fourth suspension, i.e., suspension IV;
[0111] Step 5: adding the suspension IV dropwise into the porous graphene dispersion (first solution) to obtain a mixed solution V; wherein the molar ratio of the precipitant sodium hydroxide to the tin source stannous chloride is 10:1; and the molar ratio of the tin source stannous chloride to the surfactant citric acid is 1:1;
[0112] Step 6: Transfer the mixed solution V to a reactor for hydrothermal reaction. The reaction temperature of the hydrothermal reaction is 200°C and the insulation time is 12 hours. After the hydrothermal reaction is completed, cool to room temperature, centrifuge, wash, and then freeze-dry for 48 hours to obtain the final product, i.e., a porous graphene / tin dioxide gas-sensitive material.
[0113] Step 7: Add ultrapure water to the final product gas-sensitive material to form a slurry, apply it on a ceramic tube, assemble it into a gas-sensitive element, and perform a gas-sensitive performance test.
[0114] Figure 2 The schematic diagram of X-ray diffraction test on gas sensitive materials is shown schematically in Figure 2 As shown in , there is an obvious diffraction peak corresponding to tin dioxide in the spectrum, but no diffraction peak of graphene is found. This may be because the characteristic peak of tin dioxide is stronger, which covers the peak of graphene.
[0115] Figure 13The schematic diagram of the gas-sensitive material prepared in Example 5 is shown schematically in FIG. Figure 13 As shown in the figure, it can be seen that flower-like tin dioxide (about 500nm in size) is evenly distributed on the porous graphene surface. Some flower-like structures transform into irregular spherical structures, and some accumulation occurs, which is not conducive to the diffusion of the test gas, thereby reducing the gas sensing performance. The test gas can be 50ppm acetone.
[0116] Figure 14 FIG2 schematically shows a schematic diagram of assembling the gas-sensitive material prepared in Example 5 into a gas-sensitive element for gas-sensitive performance testing. Figure 14 As shown in the figure, when the working temperature is 280℃, the gas sensitive response to 50ppm acetone gas is 13.5 and the response time is 9s.
[0117] The technical solution in the embodiment of the present disclosure adopts a simple metal etching method to prepare porous graphene, using porous graphene as the starting raw material, stannous chloride as the tin source, citric acid as the surfactant, sodium hydroxide as the precipitant, and 33 vol% ethanol aqueous solution as the solvent. It is kept warm for 12 hours under hydrothermal conditions of 160-200°C, cooled to room temperature, centrifuged and washed, and freeze-dried to synthesize a flower-clustered porous graphene / tin dioxide gas-sensitive composite material through a simple hydrothermal reaction; the flower-shaped tin dioxide (size of 300-500 nm) is evenly distributed on the surface of the porous graphene.
[0118] Flower-like clusters of gas-sensing materials were synthesized via a simple hydrothermal reaction. Compared to single tin dioxide and graphene / tin dioxide gas-sensing materials, the porous structure of graphene and the flower-like structure of tin dioxide significantly increase the specific surface area of the composite material. They also provide effective diffusion channels for the adsorption and desorption of the test gas, significantly improving its gas-sensing performance. Furthermore, the preparation process is simple, requiring no complex instrumentation, and is easily adaptable for industrial mass production.
[0119] In the flower-cluster-shaped gas-sensitive material prepared in the embodiment of the present disclosure, the size of the flower-shaped tin dioxide is about 200-500 nm and is evenly distributed on the surface of the porous graphene. The size and distribution of the flower-shaped tin dioxide on the surface of the porous graphene can be controlled by adjusting the hydrothermal conditions and the molar ratio of the precipitant sodium hydroxide and the tin source stannous chloride, which can better meet the requirements of the gas sensing field for gas-sensitive materials.
[0120] This exemplary embodiment also provides a device. This device can be a device generated based on the gas-sensitive material, such as a mobile phone, tablet computer, laptop computer, smart bracelet, smart watch, smart helmet, smart glasses, vehicle, robot, or any type of industrial equipment, as long as it can contain the gas-sensitive material. This exemplary embodiment does not specifically limit this.
[0121] Furthermore, the above-mentioned figures are merely illustrative of the processes included in the methods according to exemplary embodiments of the present disclosure and are not intended to be limiting. It is readily understood that the processes illustrated in the above-mentioned figures do not indicate or limit the temporal order of these processes. Furthermore, it is readily understood that these processes may be executed synchronously or asynchronously, for example, in multiple modules.
[0122] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the invention disclosed herein. This application is intended to cover any variations, uses, or adaptations of the present disclosure that follow the general principles of the present disclosure and include common knowledge or customary techniques in the art not disclosed herein. The description and examples are to be considered as exemplary only, with the true scope and spirit of the present disclosure being indicated by the appended claims.
[0123] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes can be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.
Claims
1. A method for preparing a gas-sensitive material, characterized in that: include: Using porous graphene as a starting material, ultrasonically dispersing a porous graphene ethanol aqueous solution to obtain a first solution; Using stannous chloride as a tin source, citric acid as a surfactant, and sodium hydroxide as a precipitant, the tin source, the surfactant, and the precipitant are sequentially dissolved in an ethanol aqueous solution to obtain a suspension; adding the suspension dropwise to the first solution to obtain a mixed solution; The mixed solution is transferred to a reactor for hydrothermal reaction, and after the hydrothermal reaction, it is cooled to room temperature for centrifugation, washing and freeze-drying to obtain a porous graphene / tin dioxide gas-sensitive material.
2. The method for preparing a gas-sensitive material according to claim 1, characterized in that: The molar ratio of the precipitant to the tin source is a first molar ratio, and the first molar ratio is 20:1 to 5:
1.
3. The method for preparing a gas-sensitive material according to claim 1, characterized in that: The molar ratio of the tin source to the surfactant is a second molar ratio, and the second molar ratio is 1:
1.
4. The method for preparing a gas-sensitive material according to claim 1, characterized in that: The reaction temperature of the hydrothermal reaction is 160 to 200° C., and the reaction time of the hydrothermal reaction is 6 to 18 hours.
5. The method for preparing a gas-sensitive material according to claim 1, characterized in that: The size of the tin dioxide gas-sensitive material in the porous graphene / tin dioxide gas-sensitive material is 300-500 nm, and the tin dioxide gas-sensitive material is evenly distributed on the surface of the porous graphene.
6. The method for preparing a gas-sensitive material according to claim 1, characterized in that: The freeze-drying time is 48 to 60 hours.
7. The method for preparing a gas-sensitive material according to claim 1, characterized in that: Using stannous chloride as a tin source, citric acid as a surfactant, and sodium hydroxide as a precipitant, the tin source, the surfactant, and the precipitant are sequentially dissolved in an ethanol aqueous solution to obtain a suspension, comprising: dissolving a tin source in an ethanol aqueous solution and stirring to obtain a second suspension; Dissolving a surfactant in an ethanol aqueous solution, stirring and adding dropwise to the second suspension to obtain a third suspension; The precipitant is dissolved in an ethanol aqueous solution, stirred and added dropwise to the third suspension to obtain a fourth suspension, and the fourth suspension is used as the suspension.
8. The method for preparing a gas-sensitive material according to claim 1, characterized in that: The method further comprises: The gas-sensitive material is prepared into slurry, and coated on a ceramic tube to assemble into a gas-sensitive element; The gas sensing element is subjected to a gas sensing performance test to determine the gas sensing response and response time.
9. The method for preparing a gas-sensitive material according to claim 1, characterized in that: The gas-sensing performance test of the gas-sensing element to determine the gas-sensing response and the response time includes: The gas sensing performance of the gas sensing element was tested in acetone gas at a working temperature of 280° C. to determine the gas sensing response and response time.
10. A gas-sensitive material, characterized in that: The gas-sensitive material is prepared according to the method for preparing a gas-sensitive material according to any one of claims 1 to 9.