Method for recovering heavy metals in oily sludge through hydrothermal catalytic gasification

The treatment of oil-containing sludge through hydrothermal catalytic gasification technology has solved the problems of heavy metal recycling and resource utilization in the existing technology, achieved efficient fixation of heavy metals and harmless treatment of waste liquids, and improved resource utilization efficiency.

CN119019061APending Publication Date: 2024-11-26RES INST OF XIAN JIAOTONG UNIV & SUZHOU
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310601472.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art fails to effectively treat and recover heavy metals in oil-containing sludge, resulting in environmental and health threats and fails to make full use of their resource value.

Method used

Using hydrothermal catalytic gasification technology, the reaction is carried out by mixing oil-containing sludge with alkali salt catalyst and deionized water, placing it in a supercritical water environment, gasifying the organic components and fixing heavy metals, and then cooling and collecting gas and solid products. , realize heavy metal recycling and harmless emission of waste liquid.

Benefits of technology

It has achieved efficient fixation and recycling of heavy metals in oily sludge, and harmless treatment of waste liquids, which has improved resource utilization efficiency and reduced environmental pollution risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019061A_ABST
    Figure CN119019061A_ABST
Patent Text Reader

Abstract

The invention provides a method for recovering heavy metals in oily sludge through hydrothermal catalytic gasification, which comprises the following steps: mixing the oily sludge with an alkali salt catalyst and deionized water, and stirring for a first preset time at a constant speed by using a stirrer to obtain uniformly mixed oily sludge slurry; placing the oily sludge slurry in a reaction kettle, enabling the reaction kettle to be in a supercritical water atmosphere, keeping for a second preset time, and then cooling the reaction kettle; discharging and collecting a gas product from the cooled reaction kettle through a pipeline, discharging a waste liquid, filtering and cleaning, and recovering a collected solid product to obtain heavy metal elements; the kettle type reactor adopted by the invention is simple in structure and convenient to maintain, through supercritical water catalytic gasification reaction, almost all organic components in the oily sludge are converted into hydrogen-rich gas, heavy metals are efficiently fixed and recycled, and harmless discharge of waste liquid can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of harmless treatment of oily sludge, and in particular to a method for recovering heavy metals in oily sludge by hydrothermal catalytic gasification. Background Art

[0002] A large amount of oily sludge is produced in the petroleum industry. The composition of oily sludge is complex and diverse. Improper disposal will not only seriously pollute the environment, but also threaten human health. Therefore, it is listed as hazardous waste. However, oily sludge contains a large amount of organic components and has a high potential for resource utilization. Therefore, it is necessary to explore efficient and harmless resource utilization solutions for oily sludge.

[0003] Supercritical water catalytic gasification technology is considered to have great potential in treating oily sludge. It can not only reduce the reaction temperature and ensure process safety, but also realize efficient resource utilization of oily sludge. Oily sludge contains a large amount of heavy metals. If it is directly discharged without recycling, it will cause serious harm to the ecological environment and human health. At present, no scholars have conducted in-depth research on the recovery of heavy metals by supercritical water catalytic gasification technology. Summary of the invention

[0004] In view of the problems existing in the prior art, the present invention provides a method for recovering heavy metals in oily sludge by hydrothermal catalytic gasification, which can gasify the organic components in the oily sludge into hydrogen-rich gas, and the heavy metals are fixed and recovered by inorganic minerals. At the same time, the waste liquid can be directly discharged safely.

[0005] The present invention is achieved through the following technical solutions:

[0006] A method for recovering heavy metals from oily sludge by hydrothermal catalytic gasification comprises the following steps:

[0007] S1: mixing the oily sludge, the alkali salt catalyst and the deionized water, and stirring them at a uniform speed for a first preset time with a stirrer to obtain a uniformly mixed oily sludge slurry;

[0008] S2: placing the oily sludge slurry in a reactor, placing the reactor in a supercritical water atmosphere, maintaining the reactor for a second preset time, and then cooling the reactor;

[0009] S3: The gaseous product of the cooled reactor is discharged and collected through a pipeline, the waste liquid is discharged and filtered and cleaned, and the collected solid product is recovered to obtain heavy metal elements.

[0010] Preferably, in step S1, the oily sludge, the alkali salt catalyst and the deionized water are in a mass ratio of 1:0.1-1:2-10.

[0011] Preferably, the first preset time in step S1 is 10 minutes.

[0012] Preferably, the alkali salt catalyst in step S1 includes KOH, NaOH, Ca(OH)2, K2CO3, Na2CO3 or CaCO3.

[0013] Preferably, the oily sludge in step S1 includes ground sludge, tank bottom sludge or refinery sludge.

[0014] Preferably, in step S2, the temperature of the reactor is maintained at 500-700° C., and the pressure is increased to 24-30 MPa.

[0015] Preferably, the second preset time in step S2 is 15-60 minutes.

[0016] Preferably, the cooling process of the reactor in step S2 is: first air cooling to below 300° C., and then water cooling to room temperature.

[0017] Preferably, in step S2, the reactor is placed in a supercritical water atmosphere and needs to be heated at a heating rate of about 15° C. / min.

[0018] Preferably, the heavy metal elements recovered in step S3 include copper, zinc, nickel, chromium and cadmium.

[0019] Compared with the prior art, the present invention has the following beneficial technical effects:

[0020] The invention provides a method for recovering heavy metals in oily sludge by hydrothermal catalytic gasification, comprising the following steps: mixing the oily sludge with an alkali salt catalyst and deionized water, and uniformly stirring the mixture with a stirrer for a first preset time to obtain a uniformly mixed oily sludge slurry; placing the oily sludge slurry in a reactor, so that the reactor is in a supercritical water atmosphere, and cooling the reactor after keeping the mixture for a second preset time; discharging and collecting gaseous products from the cooled reactor through a pipeline, discharging waste liquid and filtering and cleaning it, and recovering the collected solid products to obtain heavy metal elements; the kettle reactor used in the present application has a simple structure and is easy to maintain, and through supercritical water catalytic gasification reaction, almost all organic components in the oily sludge are converted into hydrogen-rich gas, heavy metals are efficiently and fixedly recovered, and waste liquid can be discharged harmlessly. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The present invention is a flow chart of a method for recovering heavy metals from oily sludge by hydrothermal catalytic gasification. DETAILED DESCRIPTION

[0022] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.

[0023] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0024] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0025] The present invention provides a method for recovering heavy metals from oily sludge by hydrothermal catalytic gasification. Figure 1 As shown, the following steps are included:

[0026] S1: mixing the oily sludge, the alkali salt catalyst and the deionized water, and stirring them at a uniform speed for a first preset time with a stirrer to obtain a uniformly mixed oily sludge slurry;

[0027] S2: placing the oily sludge slurry in a reactor, placing the reactor in a supercritical water atmosphere, maintaining the reactor for a second preset time, and then cooling the reactor;

[0028] S3: The gaseous product of the cooled reactor is discharged and collected through a pipeline, the waste liquid is discharged and filtered and cleaned, and the collected solid product is recovered to obtain heavy metal elements.

[0029] Furthermore, in step S1, the oily sludge, the alkali salt catalyst and the deionized water are in a mass ratio of 1:0.1-1:2-10.

[0030] Furthermore, the first preset time in step S1 is 10 minutes.

[0031] Furthermore, the alkali salt catalyst in step S1 includes KOH, NaOH, Ca(OH)2, K2CO3, Na2CO3 or CaCO3.

[0032] Furthermore, the oily sludge in step S1 includes ground sludge, tank bottom sludge or refinery sludge.

[0033] Furthermore, in step S2, the temperature of the reactor is maintained at 500-700° C., and the pressure is increased to 24-30 MPa.

[0034] Furthermore, the second preset time in step S2 is 15-60 minutes.

[0035] Furthermore, in step S2, the cooling process of the reactor is: first air-cooling to below 300° C., and then water-cooling to room temperature.

[0036] Furthermore, in step S2, the reactor is placed in a supercritical water atmosphere and needs to be heated at a heating rate of about 15° C. / min.

[0037] Furthermore, the heavy metal elements recovered in step S3 include copper, zinc, nickel, chromium and cadmium.

[0038] Embodiment 1:

[0039] First, 1.412g of oily sludge (the element mass percentage is carbon 16.34%, hydrogen 3.09%, nitrogen 0.62%, sulfur 0.52%; the heavy metal content is copper 150mg / kg, zinc 994mg / kg), 0.706g of Na2CO3 and 8g of deionized water are mixed in a customized quartz tube in advance, then put into a reactor, and finally sealed. After checking that the airtightness is good, heating is started. The temperature of the reactor is heated from room temperature to 550℃, and the heating rate is about 15℃ / min. After reaching the preset temperature, it is maintained for 30min; after the experiment, the reactor is first air-cooled to 300℃, and then water-cooled to room temperature; the gaseous products are discharged through pipelines and collected for analysis, and then the reactor is unloaded, the waste liquid can be directly and safely discharged, and the solid products collected after filtration and cleaning are analyzed for heavy metal elements.

[0040] Test results: The carbon gasification rate of oily sludge reached 31%, the gasification degree was low, and the full resource utilization of oily sludge was not achieved; the fixation rates of copper and zinc were 94% and 82% respectively, which basically achieved complete fixation.

[0041] Embodiment 2:

[0042] First, 1.412g of oily sludge (the element mass percentage is carbon 16.34%, hydrogen 3.09%, nitrogen 0.62%, sulfur 0.52%; the heavy metal content is copper 150mg / kg, zinc 994mg / kg), 0.706g of Na2CO3 and 8g of deionized water are mixed evenly in a customized quartz tube in advance, then put into a reactor, and finally sealed. After checking that the airtightness is good, heating is started. The temperature of the reactor is heated from room temperature to 600℃, and the heating rate is about 15℃ / min. After reaching the preset temperature, it is maintained for 30min; after the experiment, the reactor is first air-cooled to 300℃, and then water-cooled to room temperature; the gaseous products are discharged through pipelines and collected for analysis, and then the reactor is unloaded, the waste liquid can be directly and safely discharged, and the solid products collected after filtration and cleaning are analyzed for heavy metal elements.

[0043] Test results: The carbon gasification rate of oily sludge reached 48%, and the degree of gasification was still low, failing to achieve full resource utilization of oily sludge; the fixation rates of copper and zinc were 96% and 84% respectively, basically achieving complete fixation.

[0044] Embodiment 3:

[0045] First, 1.412g of oily sludge (the element mass percentage is carbon 16.34%, hydrogen 3.09%, nitrogen 0.62%, sulfur 0.52%; the heavy metal content is copper 150mg / kg, zinc 994mg / kg), 0.706g of Na2CO3 and 8g of deionized water are mixed in a customized quartz tube in advance, then put into a reactor, and finally sealed. After checking that the airtightness is good, heating is started. The temperature of the reactor is heated from room temperature to 650℃, and the heating rate is about 15℃ / min. After reaching the preset temperature, it is maintained for 30min; after the experiment, the reactor is first air-cooled to 300℃, and then water-cooled to room temperature; the gaseous products are discharged through pipelines and collected for analysis, and then the reactor is unloaded, the waste liquid can be directly and safely discharged, and the solid products collected after filtration and cleaning are analyzed for heavy metal elements.

[0046] Test results: The carbon gasification rate of oily sludge reached 74%, with a high degree of gasification, basically achieving full resource utilization of oily sludge; the fixation rates of copper and zinc were 99% and 79% respectively, basically achieving complete fixation.

[0047] Embodiment 4:

[0048] First, 1.412g of oily sludge (the element mass percentage is carbon 16.34%, hydrogen 3.09%, nitrogen 0.62%, sulfur 0.52%; the heavy metal content is copper 150mg / kg, zinc 994mg / kg), 0.706g of Na2CO3 and 8g of deionized water are mixed evenly in a customized quartz tube in advance, then put into a reactor, and finally sealed. After checking that the airtightness is good, heating is started. The temperature of the reactor is heated from room temperature to 700℃, and the heating rate is about 15℃ / min. After reaching the preset temperature, it is maintained for 30min; after the experiment, the reactor is first air-cooled to 300℃, and then water-cooled to room temperature; the gaseous products are discharged and collected through pipelines for analysis, and then the reactor is unloaded, the waste liquid can be directly and safely discharged, and the solid products collected after filtration and cleaning are analyzed for heavy metal elements.

[0049] Test results: The carbon gasification rate of oily sludge reached 88%, with a high degree of gasification, basically achieving full resource utilization of oily sludge; the fixation rates of copper and zinc were 95% and 67% respectively, and the fixation rate of zinc was significantly reduced.

[0050] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for recovering heavy metals from oily sludge by hydrothermal catalytic gasification. It is characterized in that The following steps are involved: S1: mixing the oily sludge, the alkali salt catalyst and the deionized water, and stirring them at a uniform speed for a first preset time with a stirrer to obtain a uniformly mixed oily sludge slurry; S2: placing the oily sludge slurry in a reactor, placing the reactor in a supercritical water atmosphere, maintaining the reactor for a second preset time, and then cooling the reactor; S3: The gaseous product of the cooled reactor is discharged and collected through a pipeline, the waste liquid is discharged and filtered and cleaned, and the collected solid product is recovered to obtain heavy metal elements.

2. According to claim 1, a method for recovering heavy metals from oily sludge by hydrothermal catalytic gasification, It is characterized in that In the step S1, the oily sludge, the alkali salt catalyst and the deionized water are in a mass ratio of 1:0.1-1:2-10.

3. According to claim 1, a method for recovering heavy metals from oily sludge by hydrothermal catalytic gasification, It is characterized in that The first preset time in step S1 is 10 minutes.

4. The method for recovering heavy metals from oily sludge by hydrothermal catalytic gasification according to claim 1, It is characterized in that The alkali salt catalyst in step S1 includes KOH, NaOH, Ca(OH) 2 , K 2 CO 3 、Na 2 CO 3 or CaCO 3 .

5. The method for recovering heavy metals from oily sludge by hydrothermal catalytic gasification according to claim 1, It is characterized in that The oily sludge in step S1 includes ground sludge, tank bottom sludge or refinery sludge.

6. The method for recovering heavy metals from oily sludge by hydrothermal catalytic gasification according to claim 1, It is characterized in that In step S2, the temperature of the reactor is maintained at 500-700° C., and the pressure is increased to 24-30 MPa.

7. The method for recovering heavy metals from oily sludge by hydrothermal catalytic gasification according to claim 1, It is characterized in that The second preset time in step S2 is 15-60 minutes.

8. The method for recovering heavy metals from oily sludge by hydrothermal catalytic gasification according to claim 1, It is characterized in that The cooling process of the reactor in step S2 is: first air cooling to below 300° C., and then water cooling to room temperature.

9. The method for recovering heavy metals from oily sludge by hydrothermal catalytic gasification according to claim 1, It is characterized in that In step S2, the reactor is placed in a supercritical water atmosphere and needs to be heated at a heating rate of about 15° C. / min.

10. The method for recovering heavy metals from oily sludge by hydrothermal catalytic gasification according to claim 1, It is characterized in that The heavy metal elements recovered in step S3 include copper, zinc, nickel, chromium and cadmium.

Citation Information

Cited By

  • Method for preparing adsorption catalytic composite material by synergistically utilizing waste incineration fly ash and printing and dyeing sludge as well as product and application of adsorption catalytic composite material

    CN120285954A

  • Method for preparing adsorption catalytic composite materials by synergistically utilizing waste incineration fly ash and printing and dyeing sludge, and its products and applications