Phase change concrete and preparation method thereof
By adding composite phase change materials to concrete and regulating temperature changes, the problem of freeze-thaw damage in concrete in cold regions has been solved, and the freeze-thaw resistance and durability of concrete have been improved.
Patent Information
- Application Number
- CN202410848834.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-26
AI Technical Summary
Existing technologies cannot effectively solve the problem of freeze-thaw damage to concrete in cold regions. Conventional methods, while reducing freeze-thaw expansion stress or increasing the critical value of tensile stress at failure, still result in concrete damage and are costly or environmentally unfriendly.
Phase change concrete is used by adding composite phase change aggregates, including n-decanoic acid, n-octanoic acid, n-tetradecane and nano-graphite, combined with fly ash ceramsite and PVA solution and cement slurry encapsulation, to form a phase change material with a low melting point, thereby regulating temperature changes and slowing down the rate of freeze-thaw cycles.
It effectively reduces the temperature fluctuation range of concrete under freeze-thaw cycles, extends service life, reduces freezing and frost damage, and improves the freeze-thaw resistance and durability of concrete.
Smart Images

Figure CN119019130A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to phase change concrete and a preparation method thereof. Background Art
[0002] At present, for concrete in cold areas, there are two necessary conditions for freeze-thaw damage: one is water infiltration to make it reach a certain saturation state, and the other is the alternation of positive and negative temperatures. Since the alternation of positive and negative temperatures and the migration of water in cold areas are inherent natural phenomena and cannot be changed, and concrete itself is a porous material, it will inevitably be affected by freeze-thaw cycles under changes in humidity and temperature. The current method of enhancing frost resistance can no longer further eliminate the impact of freeze-thaw damage on concrete. Summary of the invention
[0003] The main purpose of the present invention is to provide a phase change concrete and a preparation method thereof, aiming to solve the problem that concrete is prone to freeze-thaw damage in cold areas.
[0004] To achieve the above object, the present invention provides a phase change concrete and a preparation method thereof, wherein the materials of the phase change concrete include composite phase change aggregate and fly ash, wherein the materials of the composite phase change aggregate include n-decanoic acid, n-octanoic acid, n-tetradecane and nano-graphite.
[0005] In some embodiments, the composite phase change aggregate includes fly ash ceramsite; and / or,
[0006] The composite phase change aggregate also includes PVA solution and cement slurry.
[0007] In some embodiments, the PVA solution includes PVA powder and water, wherein the mass ratio of the PVA powder to the water is (0.1-0.12):(0.88-0.9); and / or the cement slurry includes cement powder and water, wherein the mass ratio of the cement powder to the water is (0.5-0.55):1.
[0008] The phase change concrete comprises a composite phase change aggregate, the materials of the composite phase change aggregate comprise n-decanoic acid, n-octanoic acid, n-tetradecane and nano-graphite, the composite phase change aggregate further comprises fly ash ceramsite, the composite phase change aggregate further comprises PVA solution and cement slurry, wherein the preparation method of the composite phase change aggregate comprises the following steps:
[0009] S10, mixing n-decanoic acid, n-octanoic acid, n-tetradecane and nano-graphite, and performing a first heating and stirring to obtain a first phase change material;
[0010] S20, mixing the first phase change material with fly ash ceramsite, and performing a second water bath heating and stirring to obtain a second phase change material;
[0011] S30, mixing the second phase change material, the PVA solution and cement slurry to obtain a composite phase change aggregate.
[0012] The steps of step S10 include:
[0013] S101, mixing n-decanoic acid and n-octanoic acid, heating and stirring to obtain a binary phase change material;
[0014] S102, mixing the binary phase change material with n-tetradecane, heating and stirring, to obtain a ternary phase change material;
[0015] S103, mixing the ternary phase change material and nanographite, heating and stirring, to obtain a first phase change material.
[0016] In some embodiments, in step S101, the mass ratio of the n-decanoic acid to the n-octanoic acid is (2-4):(6-8); and / or, in step S101, the heating and stirring temperature is 55-65° C., and the heating and stirring time is 50-70 min; and / or,
[0017] In step S102, the mass ratio of the binary phase change material to the n-tetradecane is (6-7):(3-4); and / or,
[0018] In step S102, the heating and stirring temperature is 35-45°C and the heating and stirring time is 50-70 minutes; and / or,
[0019] In step S103, the mass ratio of the ternary phase change material to the nanographite is 100:(3-6); and / or,
[0020] In step S103, the temperature of heating and stirring is 35-45° C., and the time of heating and stirring is 100-140 min; and / or,
[0021] In step S20, the mass ratio of the first phase change material to the fly ash ceramsite is (2-3):5.
[0022] In some embodiments, the phase change concrete further includes coarse aggregate, fine aggregate, cementitious material, water, and polycarboxylate water reducer.
[0023] In some embodiments, the coarse aggregate comprises crushed stone; and / or, the fine aggregate comprises sand and gravel; and / or, the cementitious material comprises Portland cement.
[0024] In some embodiments, the fly ash is added in an amount of 15% to 45%; and / or the composite phase change aggregate is added in an amount of 10% to 30%.
[0025] The present invention also provides a method for preparing phase change concrete, wherein the phase change concrete comprises crushed stone, sand, silicate cement, composite phase change aggregate, water, polycarboxylate water reducer and fly ash, and comprises the following preparation steps: mixing crushed stone, sand, silicate cement, composite phase change aggregate, water, polycarboxylate water reducer and fly ash to obtain a mixture, stirring the mixture, pouring the mixture into a test mold, and curing for 28 days under the conditions of 20-25° C. and a humidity of 87-97%, and then removing the mold to form the mixture to obtain the phase change concrete.
[0026] In the technical solution provided by the present invention, n-decanoic acid, n-octanoic acid, n-tetradecane and nanographite are added to the phase change concrete. The first three materials are all organic phase change materials, with stable chemical properties, high latent heat of phase change, non-toxic, and the three materials have a good eutectic effect, which is suitable for preparing phase change energy storage materials, and nanographite can be used as an additive to improve thermal conductivity, improve the thermal performance of energy storage phase change materials. After the three phase change materials are eutectic, the melting point is close to zero degrees, and the phase change can be triggered when the ambient temperature approaches the freezing point, slowing down the rate of alternating positive and negative temperature of the material. The freeze-thaw damage of concrete is closely related to the rate of change of temperature, so these phase change materials are applied to concrete and fly ash is added to make low-temperature phase change concrete, so that the phase change concrete can store and release heat as the temperature of the external environment changes. Then the temperature control of the concrete structure in the cold environment is realized, and the freezing and freezing damage of the concrete caused by low temperature is delayed and reduced, thereby improving the service life of the concrete. This method of using phase change materials to reduce the temperature change amplitude of concrete under freeze-thaw cycle conditions can fundamentally reduce the damage caused by freeze-thaw effects, effectively increase the service life of phase change concrete, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The test result diagram of the slump of concrete prepared in the test examples R-1 to A-12 of the present invention;
[0028] Figure 2 The failure modes of the cube compression test of some test cases;
[0029] Figure 3 Figure 1. Test results of the cube compressive strength of the concrete prepared for the test example;
[0030] Figure 4 A graph showing the test results of the cube compressive strength growth rate of the concrete prepared for the test example;
[0031] Figure 5 The splitting tensile failure morphology diagrams of some test cases;
[0032] Figure 6 The splitting tensile failure cross-section diagrams of some test cases;
[0033] Figure 7 Figure 2 is a graph showing the test results of the splitting tensile strength of the concrete prepared for the test example;
[0034] Figure 8 The test result diagram of the splitting tensile strength growth rate of the concrete prepared for the test example;
[0035] Fig. 9 It is the fitting relationship diagram of concrete specimen cube compressive strength and splitting tensile strength;
[0036] Fig.10 This is the layout diagram of the displacement gauge used in the axial compression test;
[0037] Fig.11 Axial compression failure morphology of concrete prepared for the test case;
[0038] Fig.12 A graph showing the test results of the axial compressive strength of the concrete prepared for the test example;
[0039] Fig.13 It is the fitting surface diagram of the content of composite phase change aggregate, fly ash content and axial compressive strength;
[0040] Fig.14 Linear relationship diagram between axial compressive strength and cube compressive strength of concrete prepared for the test case;
[0041] Fig.15 Full stress-strain graph of the concrete prepared for the test case;
[0042] Fig.16 The fitting diagram of the stress-strain constitutive curve of concrete under axial compression was prepared for the R-1 group test case;
[0043] Fig.17 The fitting diagram of the stress-strain constitutive curve of concrete under axial compression was prepared for the test case of group A-1;
[0044] Fig.18 The fitting diagram of the stress-strain constitutive curve of concrete under axial compression was prepared for the test case of group A-2;
[0045] Fig.19 The fitting diagram of the stress-strain constitutive curve of concrete under axial compression was prepared for the test case of group A-3;
[0046] Fig. 20 The fitting diagram of the stress-strain constitutive curve of concrete under axial compression was prepared for the test case of group A-4;
[0047] Fig.21 The fitting diagram of the stress-strain constitutive curve of concrete under axial compression was prepared for the test case of group A-5;
[0048] Fig. 22 The fitting diagram of the stress-strain constitutive curve of concrete under axial compression was prepared for the test case of group A-6;
[0049] Fig.23 The fitting diagram of the stress-strain constitutive curve of concrete under axial compression was prepared for the test case of group A-7;
[0050] Fig.24 The fitting diagram of the stress-strain constitutive curve of concrete under axial compression was prepared for the test case of group A-8;
[0051] Fig.25 The fitting diagram of the stress-strain constitutive curve of concrete under axial compression was prepared for the test case of group A-9;
[0052] Fig.26 The fitting diagram of the stress-strain constitutive curve of concrete under axial compression was prepared for the test case of group A-10;
[0053] Fig. 27 Fitting diagrams of the stress-strain constitutive curves of concrete under axial compression were prepared for test cases in groups A-11 and A-12. DETAILED DESCRIPTION
[0054] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.
[0055] Concrete structures in cold regions are subject to freeze-thaw cycles all year round under drastic changes in humidity and temperature, causing damage, collapse and cracking of the structures, which seriously affects the service life of the structures. Therefore, improving the frost resistance of concrete has always been the focus of research in the field of structures. Currently, the methods for improving the frost resistance of concrete are mainly concentrated in three aspects:
[0056] ① Improve the internal pore characteristics of concrete, such as reducing the water-cement ratio, adding air-entraining agents, adding volcanic ash active aggregates, adding nanomaterials or water-absorbent resins, etc.
[0057] ② Improve the tensile strength and crack resistance of concrete, such as adding various fibers or modified particles.
[0058] ③ Increase the working temperature of concrete, such as pre-burying heating pipes inside.
[0059] The above three methods can improve the frost resistance of concrete. The first two belong to "passive" methods, that is, after the concrete freezes and thaws, the freeze-thaw expansion stress is reduced or the critical value of tensile stress at failure is increased, but the freeze-thaw cycle is not really eliminated. Therefore, even if the above methods are used for reinforcement, the concrete will still suffer considerable freeze-thaw damage. In addition, these two methods also have great limitations. For example, excessive volcanic ash aggregate added to concrete will reduce the early hydration activity and reduce the strength of concrete; and excessive fiber added to concrete will flocculate and be difficult to disperse, causing holes in the concrete, seriously affecting its performance. Although the third method can effectively improve the frost resistance of concrete, it is costly and not environmentally friendly, and it is difficult to promote in actual projects. It can be seen that the commonly used methods for enhancing the frost resistance of concrete have exposed great limitations, and a new method is urgently needed to expand the prospects of research on enhancing the frost resistance of concrete.
[0060] In view of this, the present invention provides a phase change concrete and a preparation method thereof, wherein the materials of the phase change concrete include composite phase change aggregate and fly ash, wherein the materials of the composite phase change aggregate include n-decanoic acid, n-octanoic acid, n-tetradecane and nano-graphite.
[0061] It should be noted that the intensity of freeze-thaw damage is linked to the rate of temperature change. The faster the temperature change rate, the faster the water in the concrete crystallizes or melts, and the greater the frost heave stress generated. Therefore, reducing the temperature change rate is of great significance to reducing the frost damage to concrete.
[0062] In the technical solution provided by the present invention, n-decanoic acid, n-octanoic acid, n-tetradecane and nanographite are added to the materials of the composite phase change aggregate. The first three materials are all organic phase change materials, with stable chemical properties, high latent heat of phase change, non-toxic, and the eutectic effect of the three materials is very good. The melting point of the three phase change materials after eutectic is very close to zero degrees, and the phase change can be triggered when the ambient temperature approaches the freezing point, thereby slowing down the rate of positive and negative temperature alternation, which is suitable for preparing phase change energy storage materials. Nanographite can be used as an additive to improve thermal conductivity, improve the efficiency of the thermal performance of energy storage phase change materials, and the composite material can further slow down the positive and negative temperature alternation. Freeze-thaw damage is closely related to the rate of temperature change, so low-temperature phase change materials are applied to phase change concrete to make low-temperature phase change concrete, which can make the phase change materials inside the concrete store and release energy as the external environment temperature changes, thereby realizing the temperature control of the phase change concrete structure in a cold environment, delaying and reducing the freezing and freezing damage of concrete caused by low temperature, thereby improving the service life of concrete. This method of using phase change materials to reduce the temperature variation of concrete during freeze-thaw cycles can fundamentally reduce the damage caused by freeze-thaw cycles and effectively increase the service life of phase change concrete, and has broad application prospects.
[0063] In some embodiments, the composite phase change aggregate includes fly ash ceramsite. The present invention uses spherical fly ash ceramsite as a carrier of the composite phase change energy storage material. Before use, the fly ash ceramsite needs to be dried at a constant temperature of 95 to 105°C for 24 hours. The concrete obtained by adding the dried aggregate to the composite phase change aggregate can improve the internal microstructure of the phase change concrete, reduce the generation and expansion of cracks, improve the crack resistance of the phase change concrete, and extend the service life of the phase change concrete. In addition, its pore structure can reduce the thermal conductivity of the phase change concrete.
[0064] In some embodiments, the composite phase change aggregate includes a PVA solution and a cement slurry, and the PVA solution and the cement slurry are used as packaging materials for two times of packaging to complete the complete packaging of the composite phase change aggregate. These two packaging materials have good film-forming properties, can completely cover the aggregate and fill the holes on the surface, enhance the bonding effect with the external slurry, and thus greatly improve the leakage problem of the liquid phase change material.
[0065] Furthermore, the PVA solution includes PVA powder and water, and the mass ratio of PVA powder to water is (0.1-0.12): (0.88-0.9); the cement slurry includes cement powder and water, and the mass ratio of cement powder to water is (0.5-0.55): 1. Within this range, the encapsulation effect is better.
[0066] In some embodiments, the materials of the composite phase change aggregate include n-decanoic acid, n-octanoic acid, n-tetradecane and nano-graphite, the composite phase change aggregate also includes fly ash ceramsite, the composite phase change aggregate also includes PVA solution and cement slurry, and the preparation method of the composite phase change aggregate includes the following steps: S10, mixing n-decanoic acid, n-octanoic acid, n-tetradecane and nano-graphite, and performing a first heating and stirring to obtain a first phase change material.
[0067] In some embodiments, step S10 includes: compounding n-decanoic acid, n-octanoic acid, and n-tetradecane, mixing and stirring with nano-graphite, performing a first heating and stirring, the heating temperature is 35-45° C., and the stirring time after adding nano-graphite is continued for 100-140 minutes. Within this range, the mixture is evenly mixed to obtain a first phase change material.
[0068] Further, the step S10 includes: S101, mixing n-decanoic acid and n-octanoic acid, heating and stirring to obtain a binary phase change material;
[0069] S102, mixing the binary phase change material with n-tetradecane, heating and stirring, to obtain a ternary phase change material; S103, mixing the ternary phase change material with nanographite, heating and stirring, to obtain a first phase change material.
[0070] Furthermore, in step S101, the mass ratio of the decanoic acid to the octanoic acid is (2-4):(6-8), wherein the change in the component ratio will only lead to the change in the phase change temperature and the phase change latent heat. The selection principle is to give priority to the mixing ratio with a temperature closest to zero degrees, that is, the minimum eutectic point. The phase change temperature of other mixing ratios will be too high.
[0071] In step S101, the heating and stirring temperature is 55-65°C and the heating and stirring time is 50-70 minutes. Within this heating and stirring range, the n-decanoic acid and n-octanoic acid are evenly mixed and the reaction effect is good.
[0072] In step S102, the mass ratio of the binary phase change material to the n-tetradecane is (6-7):(3-4). The n-tetradecane is added here to increase the latent heat of the composite phase change material so that the phase change temperature of the composite phase change material is close to zero degrees.
[0073] In step S102, the heating and stirring temperature is 35-45°C, and the heating and stirring time is 50-70 minutes. Within this heating and stirring range, the binary phase change material and n-tetradecane are evenly mixed, and the reaction effect is good.
[0074] In step S103, the mass ratio of the ternary phase change material to the nanographite is 100:(3-6). Nanographite is added here because it has nano-sized graphite particles or graphite sheets. Due to its special structure and morphology, nanographite has excellent thermal conductivity. When combined with the ternary phase change material, the volatilization efficiency of its thermal performance can be improved.
[0075] In step S103, the heating and stirring temperature is 35-45°C and the heating and stirring time is 100-140 minutes. Within this heating and stirring range, the ternary phase change material is well compounded with the nanographite to obtain the first phase change material.
[0076] Specifically, the operation steps of step S10 include: mixing n-decanoic acid and n-octanoic acid in a mass ratio of (2-4): (8-6) and heating and stirring, the heating temperature is 55-65°C, the stirring time is 50-70min, to obtain a binary phase change material, mixing a binary phase change material in a mass ratio of (6-7): (4-3) with n-tetradecane, and stirring, the heating temperature is 35-45°C, the stirring time is 50-70min, to obtain a ternary phase change material, mixing a ternary phase change material in a mass ratio of 100: (3-6) with nanographite, heating the temperature is 35-45°C, and the stirring time is 100-140min to obtain a first phase change material.
[0077] S20, mixing the first phase change material with fly ash ceramsite, and performing a second water bath heating and stirring to obtain a second phase change material.
[0078] In some embodiments, fly ash ceramsite is an artificial composite phase change aggregate made of fly ash as the main raw material, with an appropriate amount of lime (or carbide slag), gypsum, admixtures, etc., and is made through metering, batching, molding, hydration and hydrothermal synthesis reaction or natural hydraulic reaction. It has multifunctional characteristics such as light weight, corrosion resistance, frost resistance, earthquake resistance and good insulation (heat preservation, heat insulation, sound insulation, moisture insulation), and the like. The first phase change material is mixed with fly ash ceramsite to encapsulate the first phase change material.
[0079] In some embodiments, the mass ratio of the first phase change material to the fly ash ceramsite is (2-3):5. Since the first phase change material is liquid, the fly ash ceramsite is used to adsorb the first phase change material, and the adsorption effect is good. If the mass ratio of the fly ash ceramsite is too high, the pores of the ceramsite may not be fully adsorbed, and the effect may be reduced. If the mass ratio of the fly ash ceramsite is too low, there will be too much phase change material, resulting in waste. Therefore, within this parameter range, the adsorption effect is better.
[0080] Specifically, the step S20 includes: selecting spherical fly ash ceramsite as a composite phase change energy storage material carrier, drying the carrier at a constant temperature of 95-105°C for 24 hours before use, mixing the first phase change material and the fly ash ceramsite in a mass ratio of (2-3):5 to soak the two materials, and heating and stirring the mixed material in a water bath at 40°C and 30r / min to complete the adsorption of the composite phase change energy storage material, filtering out the fly ash ceramsite after adsorption, and drying the surface to obtain the second phase change material.
[0081] S30, mixing the second phase change material, the PVA solution and cement slurry to obtain a composite phase change aggregate.
[0082] In some embodiments, PVA solution and cement slurry are prepared respectively, and the PVA solution and the cement slurry are respectively used as the first encapsulation layer and the second encapsulation layer of the composite phase change aggregate for encapsulation. Double encapsulation can improve the leakage problem, thereby preventing the adsorbed composite phase change material from leaking and improving the bonding effect between the composite phase change aggregate and the concrete matrix. The second phase change material is soaked in the order of PVA solution first and then cement slurry for 1 hour, and then filtered out and the surface is dried to obtain a composite phase change aggregate, wherein the mass ratio of the second phase change material to the encapsulation material is in the range of (13:50) to (9:25), and the encapsulation effect is optimal.
[0083] Specifically, the operation steps of S30 include: mixing PVA powder and water in a mass ratio of (0.1-0.12): (0.88-0.9) to obtain a PVA solution, and mixing cement powder and water in a mass ratio of (0.5-0.55): 1 to obtain cement slurry as a packaging material. In the order of first PVA solution and then cement slurry, the second phase change material is soaked in it for 1 hour and then filtered out and the surface is dried to obtain a composite phase change aggregate.
[0084] The present invention provides a phase change concrete, comprising coarse aggregate, fine aggregate, cementitious material, water, polycarboxylate water reducer and the composite phase change aggregate as described in any one of the above items, or the composite phase change aggregate prepared by the preparation method of the composite phase change aggregate as described in any one of the above items. The phase change concrete has all the beneficial effects of the composite phase change aggregate as described above, which will not be described one by one here.
[0085] Further, the coarse aggregate includes crushed stone; and / or, the fine aggregate includes sand and gravel; and / or, the cementitious material includes silicate cement.
[0086] Furthermore, the fly ash content is 15% to 45%; the fly ash content refers to the replacement amount of cement in concrete using an equal mass. When the fly ash content is in the range of 15% to 45%, the prepared phase change concrete has the best working performance. Among them, the composite phase change aggregate content is 10% to 30%, and the composite phase change aggregate content refers to the replacement amount of gravel in concrete using an equal volume.
[0087] The present invention also provides a method for preparing phase change concrete, wherein the phase change concrete comprises crushed stone, sand, silicate cement, composite phase change aggregate, water, polycarboxylate water reducer and fly ash, and comprises the following preparation steps: mixing crushed stone, sand, silicate cement, composite phase change aggregate, water, polycarboxylate water reducer and fly ash to obtain a mixture, stirring the mixture, pouring the mixture into a test mold, curing for 28 days under the conditions of 20-25° C. and 87-97% humidity, and then removing the mold to form the phase change concrete. The preparation method has all the beneficial effects of the composite phase change aggregate described above, which will not be repeated here one by one. Through the above steps The prepared phase change concrete, since composite phase change aggregate and fly ash are added therein, can be used to make low-temperature phase change concrete by applying the composite phase change aggregate to the phase change concrete, so that the phase change material inside the phase change concrete can store and release energy as the external ambient temperature changes, thereby realizing temperature control of the phase change concrete structure in a cold environment, delaying and reducing the freezing and frost damage of the phase change concrete caused by low temperature, thereby increasing the service life of the phase change concrete. This method of using phase change materials to reduce the temperature change amplitude of the freeze-thaw cycle of the phase change concrete can fundamentally reduce the damage caused by the freeze-thaw cycle.
[0088] Exemplarily, in some embodiments, the mass ratio of the crushed stone, the sand, the silicate cement, the composite phase-change aggregate, the water, and the polycarboxylate water-reducing agent is 11:13:15:5:3.2:0.16.
[0089] Specifically, the present application provides a phase change concrete, wherein the preparation steps of one embodiment include:
[0090] 1) Weigh cement, sand, gravel, composite phase change aggregate, water and polycarboxylate water reducer according to the mass ratio of 11:13:15:5:3.2:0.16;
[0091] 2) Put cement, sand and stone into a mixer and dry mix for 40 seconds;
[0092] 3) Add 1 / 2 of water and continue stirring for 1 minute;
[0093] 4) Add polycarboxylate water reducer and stir for 1 minute;
[0094] 5) Add composite phase change aggregate and remaining water, continue stirring for 2 minutes and measure the slump;
[0095] 6) Discharge the mixed phase change concrete and pour it into a test mold to form it;
[0096] 7) Vibrate the molded test mold for 10s to 30s. During this period, use a ash board to press the composite phase change aggregate floating on the surface into the phase change concrete, or use a surface vibrator to re-vibrate the mortar so that it returns to the surface before plastering;
[0097] 8) After the forming test mold is prepared for 1 day, the mold can be removed to obtain the test block, and then the test block is placed in the curing room for curing. The curing conditions are curing for 28 days at a temperature of 20-25°C and a humidity of 92±5% to obtain phase change energy storage phase change concrete.
[0098] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0099] Example 1
[0100] This embodiment provides a phase change concrete, wherein each portion is a unit of measurement of 1g, the composite phase change aggregate comprises the following components: n-decanoic acid, n-octanoic acid, n-tetradecane and nano-graphite, wherein the preparation method of the composite phase change aggregate comprises the following steps:
[0101] S10, heating n-decanoic acid and n-octanoic acid at a mass ratio of 1:3 at 60° C. for 60 min to obtain a binary phase change material;
[0102] The binary phase change material and n-tetradecane are heated at 40° C. for 60 min with a mass ratio of 2:1 and stirred to obtain a ternary phase change material;
[0103] The ternary phase change material and nanographite are heated at a mass ratio of 100:3 at 40° C. for 120 minutes and stirred to obtain a first phase change material;
[0104] S20, first drying the fly ash ceramsite at a constant temperature of 100° C. for 24 hours, then mixing and soaking the first phase change material and the fly ash ceramsite at a mass ratio of 2:5, and stirring at 40° C. at a speed of 30 r / min to obtain a second phase change material;
[0105] S30, respectively preparing a PVA solution and a cement slurry, wherein the PVA solution is obtained by mixing PVA powder and water in a mass ratio of 0.1:0.88 to obtain a PVA solution, and the cement slurry is obtained by mixing cement and water in a mass ratio of 0.5:1 to obtain a cement slurry, firstly mixing the second phase change material with the PVA solution for a first packaging, and then mixing it with the prepared cement slurry for a second packaging to obtain a composite phase change aggregate; the preparation method of the phase change concrete comprises the following steps:
[0106] 1) mixing the composite phase change aggregate prepared in step S30 with crushed stone, sand, silicate cement, water, polycarboxylate water reducer and fly ash to obtain a mixture, wherein cement, fly ash, sand, gravel, composite phase change aggregate, water and polycarboxylate water reducer are weighed according to a mass ratio of 15:2:20:30:2:5:0.3;
[0107] 2) Put cement, sand and stone into a mixer and dry mix for 40 seconds;
[0108] 3) Add 1 / 2 of water and continue stirring for 1 minute;
[0109] 4) Add polycarboxylate water reducer and stir for 1 minute;
[0110] 5) Add composite phase change aggregate and remaining water, stir continuously for 2 minutes and measure the slump;
[0111] 7) Discharge the mixed phase change concrete and pour it into a test mold to form it;
[0112] 8) Vibrate the molded test mold for 10s to 30s. During this period, use a ash board to press the composite phase change aggregate floating on the surface into the phase change concrete, or use a surface vibrator to re-vibrate the mortar so that it returns to the surface before plastering;
[0113] 9) After the molded test mold is prepared for 1 day, the mold can be removed to obtain the test block, and then the test block is placed in the curing room for curing. The curing conditions are as follows: curing for 28 days at a temperature of 20-25°C and a humidity of 87-97% to obtain phase change energy storage phase change concrete, that is, A-4 in Table 2.
[0114] Embodiments 2 to 9 are different from Embodiment 1 in that the method for preparing the phase change concrete comprises the following steps: the amount of the composite phase change aggregate added to the mixture is different or the amount of the fly ash added to the mixture is different, as shown in Table 2, and the rest is similar to Embodiment 1.
[0115] Comparative Example 1 is a phase change concrete, which is different from Example 1 in that fly ash and composite phase change aggregate are removed, namely R-1 in Table 2.
[0116] Comparative Example 2 is a phase change concrete, which is different from Example 1 in that fly ash is removed and the addition amount of composite phase change aggregate is 10%, that is, A-1 in Table 2.
[0117] Comparative Example 3 is a phase change concrete, which is different from Example 1 in that fly ash is removed and the addition amount of composite phase change aggregate is 20%, that is, A-2 in Table 2.
[0118] Comparative Example 4 is a phase change concrete, which is different from Example 1 in that fly ash is removed and the addition amount of composite phase change aggregate is 30%, that is, A-3 in Table 2.
[0119] Comparative Example 5 is a phase change concrete, which is different from Example 1 in that the composite phase change aggregate is removed and the amount of fly ash added is 15%, that is, R-2 in Table 2.
[0120] Comparative Example 6 is a phase change concrete, which is different from Example 1 in that the composite phase change aggregate is removed and the amount of fly ash added is 30%, that is, R-3 in Table 2.
[0121] Comparative Example 7 is a phase change concrete, which is different from Example 1 in that the composite phase change aggregate is removed and the amount of fly ash added is 45%, that is, R-4 in Table 2.
[0122] Performance testing and results
[0123] The composite phase change aggregates prepared in Examples 1 to 9 and Comparative Examples 1 to 7 were prepared into experimental phase change concrete.
[0124] The preparation steps of the phase change concrete are as follows:
[0125] 1. Preparation: Before the test, in order to ensure the accuracy of the test and reduce the water content of the sand and the mud content of the gravel, the gravel should be cleaned with clean water. The sand and gravel should be dried in a drying box. The raw materials should be weighed using an electronic balance with an accuracy of 0.01kg.
[0126] 2. Mold: This test uses a plastic mold. Before preparing the test block, the mold should be prepared and cleaned with a clean rag. In order to smoothly remove the test block, a release agent should be brushed inside the mold. Two molds were prepared for this test, namely 100*100*100 (mm) and 100*100*300 (mm) plastic molds. The molds used in the splitting tensile strength test and cube compressive strength test of phase change concrete are 100*100*100 (mm) triple plastic molds, and the mold used in the axial compressive strength test of phase change concrete is a 100*100*300 (mm) plastic mold.
[0127] 3. Mix ratio design: The physical and mechanical properties of the composite phase change aggregates prepared in Examples 1 to 9 and Comparative Examples 1 to 7 were tested and compared with gravel and fly ash ceramsite. The physical and mechanical properties of the three aggregates are shown in Table 1. It should be noted that fly ash ceramsite refers to fly ash ceramsite without adsorption of composite phase change material, and composite phase change aggregate refers to composite phase change aggregate after adsorption of composite phase change material and encapsulation with two encapsulation materials (PVA solution and cement slurry).
[0128] Table 1 Physical and mechanical properties of three aggregates
[0129]
[0130]
[0131] 4. Prepare phase change concrete test blocks: weigh the corresponding materials according to Table 2, put cement, sand and gravel into the mixer and dry mix for 1 minute, then add 1 / 2 of the water and stir for 1 minute, then add the remaining water mixed with water reducer and phase change ceramsite into the mixer and continue stirring for 2 minutes to obtain uniform phase change concrete. After the mixing is completed, put the mixture into the test mold brushed with release agent, and use a vibration table to vibrate the mold with the mixture for 10 to 30 seconds to make the phase change concrete uniform and dense. Stop vibrating immediately after the surface is uniform to prevent excessive composite phase change aggregate from floating up. After the test block is formed, it is appropriate to use a ash board to press the composite phase change aggregate floating on the surface into the phase change concrete or use a vibrator to re-vibrate the surface so that the mortar returns to the surface before plastering. Finally, the test block is sprayed with water for curing at room temperature for 1 day and demolded. After demolding, the test block is placed in a curing room for curing until it is taken out at the required age for the test. The composite phase change aggregate is added to the concrete in the form of replacing crushed stone to prepare the phase change concrete for the test. Examples 1 to 9 and Comparative Examples 1 to 7 prepare R-1 to A-12 samples corresponding to them. The specific proportions of each group are shown in Table 2.
[0132] Table 2 Proportion of each component of phase change concrete
[0133]
[0134] 5. Demolding and curing of phase change concrete specimens: After the phase change concrete specimens have been cured in a cool environment for 24 hours, they are demolded with an air pump. During the demolding process, special attention should be paid to the strength for the integrity of the specimens, and the phase change concrete specimens should not be damaged. After demolding, the surface of the phase change concrete specimens should be cleaned with a clean rag, and the specimens should be numbered. Then the specimens should be placed in a standard curing room for curing. Note that there should be a spacing of 10 to 20 mm between the specimens. After the corresponding curing time of the phase change concrete is completed, the corresponding test is carried out.
[0135] 6. Test results: The tests include slump test, cube compressive strength test, splitting tensile strength test and axial compression test, as follows:
[0136] 6.1. Slump test:
[0137] The slump of phase change concrete of R-1 to A-12 is shown in Figure 1 , Figure 1 The horizontal axis is slump and the vertical axis is mix ratio. The composite phase change aggregate after curing will still reduce the slump of the phase change concrete, indicating that the composite phase change aggregate will still absorb part of the mixing water during mixing to slightly reduce the fluidity. Considering that the morphological effect of fly ash ceramsite has the effect of improving the fluidity of phase change concrete, it is shown that the water absorption of the encapsulated cement layer of the aggregate in this experiment plays a dominant role in the change of the slump of the phase change concrete. In addition, the added fly ash can well improve the slump reduction effect, especially when the fly ash content reaches 45%, that is, when the mass replacement of fly ash for cement in the benchmark group concrete reaches 45%, the increase in aggregate content has a very weak effect on the reduction of fluidity. This is because the addition of fly ash reduces the amount of cement, and its micro-bead effect releases the filling water between cement particles, so that the paste and the composite phase change aggregate can be better wrapped, improving the working performance of the phase change concrete.
[0138] It should be noted that the working performance of phase change concrete is an important prerequisite for its excellent mechanical properties and durability. The slump of phase change concrete can evaluate its working performance. Since the designed composite phase change aggregate has absorbed sufficient phase change materials and is placed in the curing room for 7 days after the cement layer is encapsulated, the step of pre-wetting the composite phase change aggregate is cancelled. Instead, it is taken out from the curing room and the surface is dried before use.
[0139] 6.2. Cube compressive strength test
[0140] Test method: The cubic compressive strength of phase change concrete is one of the main indicators for judging the mechanical properties of phase change concrete. In 16 groups of mix ratios, 3 phase change concrete test blocks were selected in each group to test the cubic compressive strength of phase change concrete. The size was 100*100*100 (mm), with a total of 48 blocks. The test used a pressure testing machine to test the cubic compressive strength. During the test, the phase change concrete test block was placed at the center directly below the pressure testing machine, and the loading rate of the test was 0.5MPa / s.
[0141] (1) Destruction form
[0142] The failure morphology of phase change concrete of R-1 to A-12 is shown in Figure 2: The failure morphology of some phase change concrete cubes in compression tests is shown. It can be seen that phase change concretes all show typical brittle failure characteristics of four-cornered pyramids connected inversely. This is because during the vertical pressure loading of the testing machine, the loading plate tightly constrains the upper and lower surfaces of the specimen, causing the lateral deformation in the middle of the specimen to be greater than the lateral deformation of the upper and lower surfaces. Therefore, during the compressive failure of the specimen, the initial crack appears as a vertical crack in the middle of the side of the specimen. After the initial crack appears, the vertical crack will immediately expand from the middle of the specimen to the upper and lower surface corners. Subsequently, expansion and bulging characteristics will appear in the middle of the specimen, and the specimen will suddenly fail, accompanied by splashing and peeling of composite phase change aggregate and cement debris.
[0143] At the same time, it can be found that the decrease in the amount of composite phase change aggregate replacement and the increase in the amount of fly ash replacement will make the tetrahedral pyramidal failure morphology more obvious, indicating that the more composite phase change aggregate is added, the easier it is for vertical cracks to develop at the aggregate interface, which is shown in the figure as the spalling of aggregate and cement slurry or the cracking of aggregate, causing the cracks to penetrate quickly and lead to more brittle failure. The addition of fly ash can improve this phenomenon.
[0144] (2) Cube compressive strength
[0145] Since the test block used in this experiment is a plastic mold with a size of 100*100*100 (mm), the prepared test block is not a standard test block. Therefore, according to GB / T50081-2019, the cubic compressive strength of the phase change concrete test block should be calculated by multiplying the ultimate stress of the test block by a size reduction factor of 0.95. The calculation formula for the cubic compressive strength is as follows:
[0146]
[0147] In the formula, f cu is the cube compressive strength (MPa), F max is the ultimate bearing capacity of the cube, and A is the loaded area of the cube.
[0148] The cubic compressive strength of phase change concrete of R-1 to A-12 is as follows Figure 3 As shown: Figure 3 The horizontal axis is the compressive strength, and the vertical axis is the mix ratio. Changing the replacement amount of the composite phase change aggregate and keeping other conditions the same shows that the addition of the composite phase change aggregate reduces the compressive strength of the phase change concrete cube. This is because the cement layer wrapped by the composite phase change aggregate is not as strong as the bite bond with the external cement paste as the crushed stone, and the interface is prone to cracking when subjected to pressure. At the same time, the fly ash ceramsite as the composite phase change aggregate is not as hard as the crushed stone. Even if the cracks do not start from the interface, they may split directly from the shell of the ceramsite.
[0149] from Figure 3It can be seen that when the fly ash dosage is changed and other conditions are the same, the overall strength is improved after adding fly ash. The reason is that fly ash fills the pores and improves the bonding effect at the interface between the composite phase change aggregate and the external cement slurry. Secondly, the volcanic ash activity ensures the overall late compressive strength of the phase change concrete, so the compressive strength of the phase change concrete cube is improved. However, when the replacement amount of fly ash for cement is greater than 30%, the effect will be significantly reduced. Among them, the strength of the A-7 group in the embodiment is the best, and the 28d strength is only 9.1% lower than that of the R-1 group, and the 90d strength is only 6.3% lower. The strength reduction caused by the addition of composite phase change aggregate has been well improved.
[0150] The growth rate of cube compressive strength of phase change concrete of groups R-1 to A-12 is as follows Figure 4 As shown, Figure 4 The horizontal axis is the compressive strength growth rate, and the vertical axis is the mix ratio. Figure 4 The 90-day phase change concrete cube compressive strength value under different mix ratios is 100%, and the compressive strength growth rate of each mix ratio at each stage is obtained. It can be seen that with the increase of the amount of composite phase change aggregate, the early compressive strength growth rate of phase change concrete slows down. This is because the increase in concrete pores after the addition of phase change aggregate and the water absorption of the aggregate encapsulation layer push the main growth rate of strength to the later stage. With the addition of fly ash, the early concrete compressive strength growth rate slows down further, but the later growth rate is greatly improved. This is because fly ash replaces part of the cement in the concrete, and the early hydration products are reduced, but in the later stage, thanks to its volcanic ash effect, the strength of the concrete is significantly improved.
[0151] 6.3 Splitting tensile strength test
[0152] According to the Standard for Test Methods of Mechanical Properties of Ordinary Concrete (GB / T50081-2019), the splitting tensile strength test of phase change concrete was carried out. The side of the test block when it was formed was used as the splitting pressure-bearing surface, and the phase change concrete test block was placed on the pad of the testing machine. The center of the test block and the center of the pad were aligned in a line, and the pad and pad were placed. During the test, the load was applied continuously and evenly, and the loading speed was 0.08MPa / s, and the failure load was finally recorded.
[0153] (1) Destruction form
[0154] Figure 5Including the splitting tensile failure morphology diagrams of groups R-3, A-1 and A-7, the failure morphology of the splitting tensile strength test of phase change concrete with different mix ratios is generally consistent with the failure morphology of group R-3. First, a small vertical crack is generated at the center line of the phase change concrete specimen, and quickly develops into a main crack that penetrates the upper and lower surfaces of the phase change concrete specimen. Then the phase change concrete specimen breaks into two parts. There is no obvious sign of destruction during the whole process, and the duration is not long, which is a brittle failure. Part of the fracture surface of the phase change concrete is damage along the interface of the cement stone composite phase change aggregate, which shows that compared with ordinary concrete, the bonding ability of the composite phase change aggregate and cement stone is weak. The splitting tensile strength of the specimen is a main crack that develops along the center line of the phase change concrete and penetrates the upper and lower surfaces. The difference is that the brittleness of the phase change concrete affects the development characteristics of the main crack. Figure 5 It can be seen that the cracks developed in ordinary concrete when subjected to splitting load are small and serrated, while the cracks developed in group A-1 with only 10% composite phase change aggregate are straight and wide, indicating that the brittleness has increased. The brittle characteristics of group A-7 with 10% composite phase change aggregate and 30% fly ash are weakened, and the cracks return to serrated shape and the width becomes smaller.
[0155] The splitting tensile sections of Group A-1 and Group A-7 are shown in Figure 6 As shown, Figure 6 The section of group A-1 on the left is basically carried out along the interface between the composite phase change aggregate and the phase change concrete cement paste. The composite phase change aggregate is exposed in the section, and the encapsulated cement layer and PVA layer are also peeled off and torn to varying degrees. Figure 6 The cross-sectional view of group A-7 on the right shows that the exposed composite phase change aggregate at the crack has been reduced a lot, which indicates that the addition of fly ash can better improve the interface between the composite phase change aggregate and cement paste, and better protect the integrity of the composite phase change aggregate when the phase change concrete is under load.
[0156] (2) Splitting tensile strength
[0157] Since the test block used in this experiment is a plastic mold with a size of 100*100*100 (mm), the prepared test block is not a standard test block. Therefore, according to GB / T50081-2019
[68] , the cubic splitting tensile strength of the phase change concrete test block should be calculated by multiplying the ultimate stress of the test block by a reduction factor of 0.85. The calculation formula for the splitting tensile strength is as follows:
[0158]
[0159] In the formula, f spt is the cube splitting strength (MPa), F max is the ultimate bearing capacity of the cube (kN), A is the load-bearing area of the cube (mm 2 ).
[0160] The splitting tensile strength and growth rate of phase change concrete of various mix ratios are as follows: Figure 7 and 8 As shown, Figure 7 The horizontal axis is the splitting tensile strength, and the vertical axis is the mix ratio. Figure 8 The horizontal axis is the growth rate of splitting tensile strength, and the vertical axis is the mix ratio. It can be seen that when the fly ash content and other conditions remain unchanged, as the replacement amount of composite phase change aggregate increases from 10% to 20% or even 30%, the increase in the replacement amount of composite phase change aggregate leads to a decrease in interfacial bonding. At the same time, the aggregate itself has weak anti-splitting ability, resulting in a decrease in splitting tensile strength. With the increase in the age of phase change concrete with different mix ratios, its splitting tensile strength shows an increasing phenomenon. With the increase in fly ash content, the splitting tensile strength first increases and then decreases. This is because fly ash improves the bonding strength between cement paste and composite phase change aggregate, but the improvement effect is limited, so the fly ash content should be controlled within an appropriate range. The splitting tensile strength is closely related to the strength of the bonding surface between cement paste and aggregate, so the increase in aggregate content makes it easier for cracks to split from the bonding surface, resulting in a decrease in strength. The addition of fly ash refines the pore structure at the bonding surface to a certain extent, allowing the encapsulated cement layer to be in closer contact with the cement paste of the phase change concrete itself, thereby improving the overall splitting tensile strength. Among the embodiments, the strength of group A-7 is the best, and the splitting tensile strength at 28d is only 5.22% lower than that of group R-1, and the strength at 90d is only 2.46% lower, indicating that the interface between the phase change aggregate and the cement paste in the concrete has been well improved.
[0161] (3) Relationship between cube compressive strength and splitting tensile strength
[0162] Based on formula (3.3), the nonlinear least square method was used to establish the fitting relationship between the cubic compressive strength and splitting tensile strength of the phase change concrete specimen, see Fig. 9 . Fig. 9 The linear relationship between the compressive strength and splitting tensile strength of the phase change concrete cube is fitted through a scatter plot, which can help predict the tensile strength through the compressive strength of concrete in actual engineering, which is convenient for practical application. The fitting formula is shown in the following formula (3.4). The correlation coefficient between the predicted values of the compressive strength and splitting tensile strength of the phase change concrete cube is about 0.932. The fitting accuracy meets the requirements and can be used to predict the tensile strength.
[0163]
[0164] a, b: correspond to different parameters.
[0165]
[0166] 6.3 Axial compression test
[0167] Comparative Examples R-2, R-3 and R-4 are omitted. In the remaining 13 mix ratios, 3 phase change concrete test blocks are selected from each group to test the axial compressive strength of phase change concrete. The size is 100*100*300 (mm), with a total of 39 blocks. During the test, the phase change concrete test blocks are placed at the center directly below the pressure testing machine, and the loading rate of the test is adjusted to 0.075mm / min. During the test, a YHD-50 displacement meter is used to collect vertical and lateral displacements. The displacement meter layout diagram is shown in Fig.10 .
[0168] Since the test block used in this experiment is a plastic mold with a size of 100*100*300 (mm), the prepared test block is not a standard test block. Therefore, according to GB / T50081-2019
[68] , the axial compressive strength of the phase change concrete test block should be calculated by multiplying the ultimate stress of the test block by a reduction factor of 0.95. The calculation formula of the axial compressive strength is as follows:
[0169] In the formula, f c is the axial compressive strength (MPa), F max is the ultimate bearing capacity of the cube, and A is the loaded area of the cube.
[0170] 6.1 Destruction form
[0171] The axial compression failure morphology of phase change concrete of groups R-1 to A-12 is shown in Fig.11 Generally, the axial compression failure of phase change concrete will go through four stages. In the elastic stage, the specimen deforms evenly and no visible cracks appear on the surface. In the crack development stage, after the elastic stage, as the load continues to increase, the internal cracks of the phase change concrete begin to expand and extend, and visible cracks appear on the surface. In the destruction stage, after the load exceeds the peak load, the cracks on the surface of the phase change concrete expand rapidly, and finally the cracks penetrate and cause the cross-section to be destroyed.
[0172] For the benchmark group of concrete, there was no obvious change in the test blocks at the initial stage of loading. When the loading approached the peak load, oblique microcracks suddenly appeared on the surface, and then quickly developed and expanded along the diagonal to both ends. A loud bursting sound was heard when it was destroyed, and there were very few signs of destruction. It was a typical brittle shear failure.
[0173] Fig.11In the phase-change concrete of groups A-1 to A-3, small vertical cracks appeared in the upper and middle parts of the test blocks as the load increased. After continuous loading, the cracks developed rapidly downward until they penetrated the entire cross section. When the test blocks were destroyed, they were divided into multiple thin columns by the vertical cracks, and the phase-change concrete at the top of the test blocks was crushed. This failure feature is attributed to the insufficient bonding strength between the composite phase-change aggregate and the slurry. When the test blocks are subjected to axial pressure, due to the Poisson effect, transverse tensile stress will be generated inside, and the interface between the composite phase-change aggregate and the slurry is prone to cracking under the action of tensile stress, causing the vertical cracks to penetrate the cross section, and finally the test blocks are destroyed under the action of tensile stress. This failure feature becomes more obvious with the increase of aggregate content, especially when the content of composite phase change aggregate is 30%. A large amount of composite phase change aggregate cannot be well dispersed in the phase change concrete matrix, which weakens the homogeneity of the matrix. The development of vertical cracks changes from several fine long cracks near the vertical center axis to wide cracks on the edge, indicating that the cracks penetrate and destroy from the weak points, resulting in a decrease in strength. This is also an important reason why the content of composite phase change aggregate needs to be limited.
[0174] 6.2. Axial compression failure mode
[0175] For the phase change concrete of groups R-1 to A-12, the addition of fly ash has improved the bonding effect between the composite phase change aggregate and the paste, and the main failure mode of the test block has changed. When the fly ash content is 15%, oblique cracks begin to appear at the upper corner of the test block as the load increases, and then the cracks extend to the middle and gradually expand into vertical main cracks, indicating that the bonding effect between the composite phase change aggregate and the paste has been improved to a certain extent, but the main failure feature of the test block is still tensile stress failure. When the fly ash content is 30%, the test block first has fine vertical cracks and oblique cracks in the middle, and then gradually expands and intersects. The main failure mode has turned into shear failure that penetrates the diagonal line, indicating that the addition of fly ash has achieved a good effect on the improvement of the interface at this time. At the same time, the increase in fluidity also makes the phase change concrete more homogeneous as a whole, so the strength and strain of the phase change concrete are well improved at this time. When the fly ash content is 45%, the excessive replacement of cement by fly ash causes the strength and adhesion of the paste to decrease, and the improvement effect on the composite phase change aggregate interface is also weakened, and the failure mode is converted into a failure mode in which shear failure and vertical tensile failure coexist.
[0176] 6.2.1 Axial compression strength analysis
[0177] The axial compressive strength of phase change concrete of groups R-1 to A-12 is as follows Fig.12The axial compressive strength of the ordinary concrete of group R-1 is 57.4MPa, the axial compressive strength of the phase change concrete groups A-1 to A-3 with single aggregate is 47.1MPa, 43.76MPa, and 39.3MPa respectively, and the axial compressive strength of the phase change concrete groups A-4 to A-6 with 10%, 20%, and 30% of composite phase change aggregate and 15% of fly ash is 47.49MPa, 46.3MPa, and 42.15MPa respectively. The axial compressive strength of phase change concrete groups A-7 to A-9 with 10%, 20%, 30% composite phase change aggregate and 15% fly ash is 56.54MPa, 55.89MPa, 48.39MPa, and the axial compressive strength of phase change concrete groups A-10 to A-12 with 10%, 20%, 30% composite phase change aggregate and 15% fly ash is 49.23MPa, 47.21MPa, 43.22MPa. The axial compressive strength of phase change concrete decreases with the increase of composite phase change aggregate content, indicating that composite phase change aggregate will reduce the axial compressive strength of phase change concrete. The axial compressive strength of phase change concrete increases first and then decreases with the increase of fly ash content, indicating that the addition of an appropriate amount of fly ash can improve the reduction of strength caused by composite phase change aggregate. Among them, the phase change concrete specimens of group A-7 with 10% composite phase change aggregate and 30% fly ash have the best mechanical properties, which are only 1.5% lower than those of the benchmark group.
[0178] 6.3 Axial compressive strength of phase change concrete
[0179] Based on the experimental rules, a mathematical relationship between the phase change aggregate content, fly ash content and axial compressive strength was designed:
[0180] f cp =f c (1+ax)(1+by+cy 2 ) (3.6)
[0181] In the formula, f cp is the predicted value of concrete axial compressive strength, f c is the axial compressive strength test value of the benchmark concrete, x is the phase change aggregate content, y is the fly ash content, and a, b, and c are constants. The fitting surface diagram is shown in Fig.13 . Fig.13 The phase change aggregate content and fly ash content are used as independent variables, and the axial compressive strength test value is used as the dependent variable. The mathematical model between the material content and the axial compressive strength of concrete is obtained by fitting the nonlinear relationship between the three. This is convenient for accurately predicting the strength value of concrete under the mix ratio when adjusting the concrete mix ratio in actual engineering applications to enhance construction safety. The fitting formula is shown in Formula 3.7.
[0182] 6.4 Prediction of axial compressive strength
[0183] f cp =f c (1-1.125x)(1+0.911y-1.167y 2 )R2=0.934(3.7)
[0184] Table 3 Axial compressive strength, cubic compressive strength and ratio of phase change concrete
[0185]
[0186]
[0187] The results of axial compressive strength, cubic compressive strength and the ratio of the two are shown in Table 3. It can be seen that the strength of concrete with phase change aggregate is higher than that of the baseline concrete, and its ratio increases with the increase of aggregate addition. This is because the deformation properties of concrete test blocks and steel plates are quite different. When the test blocks are compressed, the lateral friction between the steel plate and the surface of the test blocks will constrain the deformation of the test blocks, forming a hoop effect, which inhibits the expansion of cracks under lateral stress. This is why the cubic compressive strength is higher than the axial compressive strength. The concrete with the addition of composite phase change aggregate becomes lighter and has a lower elastic modulus. The hoop effect has less constraint on its lateral deformation, so the improvement of the cubic compressive strength is also smaller, making the damage state of the two closer.
[0188] From the test results, it can be seen that there is a certain linear relationship between the axial compressive strength and the cube compressive strength. For the concrete with composite phase change aggregate, the specific fitting relationship between the cube compressive strength and the axial compressive strength is shown in formula 3.8. The linear coefficient of the fitted phase change concrete strength ratio is about 0.928, which is consistent with the test analysis results. The fitting relationship between the cube compressive strength and the axial compressive strength of the test block is shown in formula 3.8. Fig.14 .and Fig. 9 Similarly, the nonlinear mathematical relationship between the axial compressive strength and the cube compressive strength can be fitted through the scatter plot. In order to obtain an accurate functional relationship, the axial compressive strength can be accurately predicted using the concrete cube compressive strength, which is convenient for actual construction applications. The fitting equation is as follows:
[0189] f c =0.928f cu R 2 =0.962 (3.8)
[0190] 6.4. Analysis of the full stress-strain curve
[0191] The stress-strain curve of phase change concrete and the test results of the characteristic points of the whole curve are shown in Fig.15Compared with Table 4, it can be seen that the addition of phase change aggregate reduces the elastic modulus, ultimate strain and stiffness, and the reduction becomes larger with the increase of aggregate content.
[0192] 6.4.1. As for the decrease of elastic modulus and stiffness, the rising section of the curve becomes steeper after adding aggregate, and some groups even show a concave rising trend. This is mainly because compared with the concrete of group R-1, the density inside the concrete is lower, and the bearing capacity increases more slowly during the deformation process. The concave rising section indicates that the interior has undergone a compaction process, and the energy dissipation capacity and deformation resistance capacity have weakened.
[0193] 6.4.2. As for the decrease of ultimate strain, after the bearing capacity exceeds the peak stress, the cracks inside the concrete begin to expand rapidly. At this time, the cracks are more likely to be destroyed at the interface between the phase change aggregate and the cement paste. Therefore, the more aggregate is added to the concrete, the steeper the descending section is, which means that the cracks develop faster and the damage is more severe in the final destruction stage.
[0194] Table 4 Full curve feature point test results
[0195]
[0196]
[0197] It can be seen from Table 4 that the addition of fly ash can better improve the reducing effect of phase change aggregate on elastic modulus, ultimate strain and stiffness, which first increases and then decreases with the increase of fly ash content, which is consistent with the test results of axial compressive strength. An appropriate amount of fly ash can strengthen the interface between aggregate and paste, increase its internal density, and make the crack development speed in the destruction stage more controllable.
[0198] 6.5. Uniaxial Compression Constitutive Fitting
[0199] The constitutive derivation is based on the uniaxial compressive stress-strain numerical model, see Formulas 3.8 to 3.11.
[0200] y=ax+(3-2a)x 2 +(a-2)x 3 , x≤1 (3.8)
[0201]
[0202] Where a and b are the parameter values of the rising and falling sections of the uniaxial compressive stress-strain curve, respectively, and ε c ' and ε c are the strain value and peak strain of concrete, σ c and f c are the stress value and peak stress of concrete respectively.
[0203] The uniaxial compression test data of phase change concrete of groups R-1 to A-12 were fitted using formulas 3.8 to 3.11. The obtained stress-strain test curves and fitting curves correspond to each other as follows: Figure 16 to Figure 27 As shown, Fig.16 For the R-1 group, Fig.17 For Group A-1, Fig.18 For Group A-2, Fig.19 For Group A-3, Fig. 20 For Group A-4, Fig.21 For Group A-5, Fig. 22 For Group A-6, Fig.23 For Group A-7, Fig.24 For Group A-8, Fig.25 For A-9, Fig.26 For the A-10 group, Fig. 27 For groups A-11 and A-12, the parameters of the rising section, the falling section and the fitting accuracy of the fitting curve are shown in Table 5.
[0204] Table 5 Stress-strain curve fitting parameters and fitting accuracy
[0205]
[0206]
[0207] Depend on Figures 16-27 It can be seen that for concrete with composite phase change aggregate, the rising section is often not as steep as that of R-1 group concrete, and due to the addition of composite phase change aggregate, the rising section of the stress-strain curve of some mix proportions of concrete is concave. At the same time, due to the bonding and strength problems of composite phase change aggregate, the rate of its falling section is higher than that of R-1 group. As shown in Table 5, after the curve is fitted using the Guo Zhenhai model, the R 2 It is above 0.89, exceeding the minimum requirement of 0.85, so it can basically meet the fitting requirements.
[0208] In summary, the following conclusions can be drawn: the concrete prepared by the present invention has the ability to control temperature at about 0°C, and has the characteristics of excellent mechanical properties, low cost and easy construction, and can be well applied to concrete projects in high-cold areas. After macroscopic testing of the designed concrete, it was concluded that the low-temperature phase change concrete has good workability and maintains good mechanical properties. Its 28d axial compressive strength is only 2.6% lower than that of the concrete in the R-1 group, and its 28d splitting tensile strength is only 5.22% lower than that of the R-1 group, which has better improved the weakening effect of phase change aggregate on concrete strength and can be well applied in engineering practice.
[0209] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A phase change concrete, characterized in that: The materials of the phase change concrete include composite phase change aggregate and fly ash, wherein the materials of the composite phase change aggregate include n-decanoic acid, n-octanoic acid, n-tetradecane and nano-graphite.
2. The phase change concrete according to claim 1, characterized in that: The composite phase change aggregate further includes fly ash ceramsite; and / or, The composite phase change aggregate also includes PVA solution and cement slurry.
3. The phase change concrete according to claim 2, characterized in that: The PVA solution comprises PVA powder and water, wherein the mass ratio of the PVA powder to the water is (0.1-0.12): (0.88-0.9); and / or, The cement slurry includes cement powder and water, and the mass ratio of the cement powder to the water is (0.5-0.55):
1.
4. The phase change concrete according to any one of claims 1 to 3, characterized in that: The phase change concrete comprises a composite phase change aggregate, the materials of the composite phase change aggregate comprise n-decanoic acid, n-octanoic acid, n-tetradecane and nano-graphite, the composite phase change aggregate further comprises fly ash ceramsite, the composite phase change aggregate further comprises PVA solution and cement slurry, wherein the preparation method of the composite phase change aggregate comprises the following steps: S10, mixing n-decanoic acid, n-octanoic acid, n-tetradecane and nano-graphite, and performing a first heating and stirring to obtain a first phase change material; S20, mixing the first phase change material with fly ash ceramsite, and performing a second water bath heating and stirring to obtain a second phase change material; S30, mixing the second phase change material, the PVA solution and cement slurry to obtain a composite phase change aggregate.
5. The phase change concrete according to claim 4, characterized in that: The steps of step S10 include: S101, mixing n-decanoic acid and n-octanoic acid, heating and stirring to obtain a binary phase change material; S102, mixing the binary phase change material with n-tetradecane, heating and stirring, to obtain a ternary phase change material; S103, mixing the ternary phase change material and nanographite, heating and stirring, to obtain a first phase change material.
6. The phase change concrete according to claim 5, characterized in that: In step S101, the mass ratio of the n-decanoic acid to the n-octanoic acid is (2-4):(6-8); and / or, In step S101, the heating and stirring temperature is 55-65° C., and the heating and stirring time is 50-70 min; and / or, In step S102, the mass ratio of the binary phase change material to the n-tetradecane is (6-7):(3-4); and / or, In step S102, the heating and stirring temperature is 35-45°C and the heating and stirring time is 50-70 minutes; and / or, In step S103, the mass ratio of the ternary phase change material to the nanographite is 100:(3-6); and / or, In step S103, the temperature of heating and stirring is 35-45° C., and the time of heating and stirring is 100-140 min; and / or, In step S20, the mass ratio of the first phase change material to the fly ash ceramsite is (2-3):
5.
7. The phase change concrete according to any one of claims 1 to 6, characterized in that: The phase change concrete also includes coarse aggregate, fine aggregate, cementitious material, water and polycarboxylate water reducing agent.
8. The phase change concrete according to claim 7, characterized in that: The coarse aggregate comprises crushed stone; and / or, The fine aggregate includes sand and gravel; and / or, The cementitious material includes silicate cement.
9. The phase change concrete according to claim 7, characterized in that: The fly ash content is 15% to 45%; and / or, The addition amount of the composite phase change aggregate is 10% to 30%.
10. A method for preparing the phase change concrete according to any one of claims 1 to 9, characterized in that: The phase change concrete comprises crushed stone, sand, silicate cement, composite phase change aggregate, water, polycarboxylate water reducer and fly ash, and comprises the following preparation steps: mixing crushed stone, sand, silicate cement, composite phase change aggregate, water, polycarboxylate water reducer and fly ash to obtain a mixture, stirring the mixture, pouring the mixture into a test mold, curing for 28 days under the conditions of 20-25° C. and 87-97% humidity, and then removing the mold to form the mixture to obtain the phase change concrete.