Vegetation concrete structure for realizing multi-spectrum compatible camouflage and preparation method thereof
By introducing porous structures, iron salt-modified absorbing materials and infrared reflective fiber webs into concrete, combined with plant seeds, multi-spectrum compatible camouflage is achieved, solving the shortcomings of traditional concrete materials in electromagnetic wave absorption and infrared stealth, and improving the The stealth performance and ecological benefits of the facility.
Patent Information
- Application Number
- CN202411029834.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Existing stealth materials are difficult to achieve multi-spectrum compatibility camouflage, especially in buildings, roads and bridges and other facilities. The electromagnetic wave reflectivity of traditional concrete materials is low and the absorption capacity is weak, so they cannot meet the current multi-spectrum, all-round, all-weather, and intelligent. The demand for stealth technology.
Using composite structures, including porous vegetation concrete, iron salt-modified absorbent lees pellets and absorbent lees biochar, infrared reflective coconut fiber web and plant seeds, through incorporation, coating and multi-layer composite technology, it forms multiple Spectrum compatible with camouflage function phytogenetic concrete.
It improves the electromagnetic absorption, reflection and scattering performance of concrete, enhances infrared and visible light stealth functions, and realizes the multi-spectrum compatibility camouflage effect of radar, infrared and visible light, and has both economical and ecological effects.
Smart Images

Figure CN119019132A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of stealth materials, and in particular to a vegetative concrete structure for realizing multi-spectrum compatible camouflage and a preparation method thereof. Background Art
[0002] At present, the research and application of stealth materials are mainly concentrated on military equipment such as ships, aircraft, and missiles. For the stealth of military facilities, camouflage nets and coatings are more often used, and research on stealth in buildings, roads, bridges, etc. is still insufficient. Concrete is a common material for facilities such as buildings, roads, and bridges. The development of stealth concrete materials and structures is of great significance to the safety of military facilities. In addition, in response to the current development trend of stealth technology of "multi-spectrum, all-round, all-weather, and intelligent", materials with a single stealth function can no longer meet market demand, and materials and structures that can achieve multi-spectrum compatible camouflage have more development potential.
[0003] Good impedance matching and attenuation characteristics are the basic conditions for materials to effectively attenuate incident electromagnetic waves. Cement has certain electromagnetic loss characteristics because it contains certain iron oxide compounds, but cement will form a dense structure after hydration reaction, which is not conducive to electromagnetic waves entering the interior of the cement material structure. Most electromagnetic waves will be reflected on the surface of the cement matrix, that is, the low ferrite content and the difficulty of electromagnetic waves entering the interior of cement-based materials are the main reasons for the low electromagnetic reflectivity of cement-based materials. Patent CN104628421A proposes a surface wave absorption modification technology for cement and concrete. Under the action of an external magnetic field, magnetic materials are infiltrated into the formed cement and concrete to form a surface layer with wave absorption performance. Patent CN109912279A discloses a foamed cement-based zeolite-ferrite wave absorbing material. By combining low-cost foamed porous cement-based materials with magnetic loss wave absorbing materials, the cost of wave absorbing materials is reduced and the performance of wave absorbing materials is improved. The above invention improves the electromagnetic wave absorbing performance of cement or concrete internal materials by adding external wave absorbing materials and improving the pore structure. The process is simple and economical, but it does not have a multi-spectrum stealth function.
[0004] In order to meet the needs of multi-band compatible camouflage of military facilities, the present invention starts from the two aspects of material combination and structure construction according to the functional characteristics of each stealth material, and integrates electromagnetic absorption materials, infrared reflection materials, visible light stealth vegetation layers and porous structures through mixing, coating and multi-layer composite, and proposes a vegetation concrete composite structure that can achieve radar, infrared and visible light multi-spectrum compatible camouflage. Summary of the invention
[0005] The purpose of the present invention is to provide a microwave-absorbing plant-based concrete that can achieve multi-spectrum compatible camouflage by combining microwave-absorbing wine grains pellets and microwave-absorbing wine grains biochar modified by iron salt with a composite structure of infrared-reflective coconut fiber net and plants.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A vegetative concrete structure for achieving multi-spectrum compatible camouflage, comprising a porous vegetative concrete with electromagnetic wave absorption function, a vegetative matrix A filled in the porous vegetative concrete with electromagnetic wave absorption and soil improvement functions, a vegetative matrix B attached to the surface of the porous vegetative concrete, and an infrared coconut fiber net with infrared reflection function laid on the porous vegetative concrete, wherein plant seeds are mixed in the vegetative matrix B, and the plant seeds grow to form a vegetation cover layer with visible light and radar stealth functions;
[0008] The porous vegetation concrete comprises the following components by mass: 100-110 parts of mixed cementitious materials, 625-670 parts of wave-absorbing wine lees aggregates, 22-37 parts of water, 10-11 parts of water reducing agent, and 2-4 parts of thickener;
[0009] The plant growth matrix A comprises the following components by mass: 6-8 parts of wave-absorbing wine lees biochar, 60-90 parts of soil, 10-20 parts of wine lees powder, 3-6 parts of mixed gelling materials, 10-20 parts of organic matter, 0.6-1 parts of compound fertilizer, 0.08-0.1 parts of water retaining agent, and 20-30 parts of water;
[0010] The planting matrix B comprises a planting matrix A and mixed planting seeds mixed in the planting matrix A, wherein the mixed planting seeds in the planting matrix A are mixed in an amount of 25-50 g / m 2 ;
[0011] The infrared coconut fiber net has a mesh size of 5*5cm, a wire diameter of 0.4-0.5cm, a strength of>0.8kN / m, and a tensile force of ≥20kg.
[0012] Furthermore, the mixed cementitious material is a mixture of L-SAC 42.5 cement and PO 42.5 cement in a mass ratio of 1:1.
[0013] Furthermore, the preparation method of the wave-absorbing wine lees pellets includes the following operations: placing wine lees waste residue with a moisture content of 25-30wt% after drying or pre-wetting treatment in a pelletizer to form wine lees pellets with a diameter of 1-1.5mm, and then placing the formed wine lees pellets in a muffle furnace under nitrogen conditions at 450°C for 4h, and modifying the pyrolyzed wine lees pellets by soaking in an iron salt solution to obtain the wave-absorbing wine lees pellets.
[0014] Furthermore, the modification of the pyrolyzed distiller's grains by soaking them in an iron salt solution includes the following operations: soaking the pyrolyzed distiller's grains in an iron salt solution with a concentration of 1 mol / L for 12-24 hours, wherein the iron salt solution is one or more of FeSO4 solution, FeCl3 solution, Fe(NO4)2 solution, and Fe(Ac)2 solution; after the distiller's grains fully absorb the iron salt solution, they are removed and drained, placed in a muffle furnace and calcined at 400-450°C for 2 hours, and then washed with deionized water and dried after calcination.
[0015] Furthermore, the preparation method of the wave-absorbing wine lees biochar includes the following operations: placing the wine lees residue in an oven at 90-100°C to dry, crushing it through a 16-18 mesh sieve, the part above the sieve is grain plant fiber, and the part below the sieve is the wine lees powder, the sieved grain plant fiber is subjected to oxygen-isolated high-temperature heating to obtain wine lees biochar, and then the wine lees biochar is soaked in an iron salt solution for modification to obtain the wave-absorbing wine lees biochar.
[0016] Furthermore, the process of preparing distiller's grain biochar by high-temperature heating the sieved cereal plant fibers in oxygen isolation comprises the following operations: placing the cereal plant fibers in a muffle furnace for anaerobically pyrolysis at 450°C under nitrogen conditions for 2 hours, grinding them through an 80-100 mesh sieve to obtain biochar; the process of modifying the distiller's grain biochar by soaking them in an iron salt solution comprises the following operations: mixing the distiller's grain biochar and the iron salt solution at a ratio of 100g / L and stirring them evenly for adsorption, wherein the iron salt solution is one or more of FeSO4 solution, FeCl3 solution, Fe(NO4)2 solution, and Fe(Ac)2 solution, with a concentration of 1mol / L, and after adsorption for 30 minutes, placing the mixture in a muffle furnace and calcining it at 400-450°C for 2 hours, and then washing and drying the mixture with deionized water after calcination.
[0017] Furthermore, the mixed vegetation seeds include the following components in percentage by mass: 20% annual herbaceous plants, 35% perennial herbaceous plants, 15% vines, 20% perennial legumes, and 10% perennial shrubs, wherein the annual herbaceous plants are one or more of ryegrass and cosmos, the perennial herbaceous plants are one or more of big wufeng grass, reed fescue, alkali grass, orchard grass, and bahia grass, the vines are one or more of parthenocissus, wild sweet potato, and ivy, the perennial legumes are one or more of red bean grass, Medicago truncatula, and glossy purple flower vetch, and the perennial shrubs are one or more of purple Sophora japonica, pigeon pea, sea buckthorn, and Lespedeza
[0018] Furthermore, the preparation method of the infrared coconut fiber net is: preparing infrared reflective paint from infrared reflective pigment, deionized water, additives, and glass beads, and then applying the infrared reflective paint to the coconut fiber net by spraying, brushing or rolling to obtain the infrared coconut fiber net.
[0019] Furthermore, the infrared reflective pigment is mixed with Cr2O3, Fe2O3, TiO2, and Al(OH)3 in a ratio of Cr:Fe:Ti:Al of 209.3:1:6.7:15.9, and then placed in a ball mill for wet mixing and grinding for 5 hours, taken out and centrifuged, dried, ground through a 200-mesh sieve, and then the sieve under the sieve is placed in a tubular atmosphere furnace, heated to 780-1080°C at a rate of 2°C / min and calcined for 3 hours to obtain the infrared reflective pigment;
[0020] The effective density of the glass microspheres is 0.32-0.40 g / cm 3 , the average particle size is 30μm, and the particle size distribution is 16-60μm;
[0021] Infrared reflective pigment, deionized water and additives are prepared into pigments and fillers in proportion, and then glass beads are added in a proportion of 9-27% by mass of the pigments and fillers to prepare infrared reflective coating; preferably, the mass ratio of infrared reflective pigment, deionized water and additives is 10:30:58, and preferably, the additives include the following components in parts by mass: 8 parts of kaolin, 24 parts of heavy calcium powder and 26 parts of AC-261P emulsion.
[0022] The present invention also provides a method for preparing a vegetation concrete structure that realizes multi-spectrum compatible camouflage, comprising the following steps:
[0023] S1. Forming 100-110 parts by weight of mixed cementitious materials, 625-670 parts by weight of lees pellets, 22-37 parts by weight of water, 10-11 parts by weight of water reducing agent, and 2-4 parts by weight of thickener into a vegetation porous concrete by a pre-coating method;
[0024] S2, 6-8 parts by mass of absorbing wine lees biochar, 60-90 parts of soil, 10-20 parts of wine lees powder, 3-6 parts of mixed cementitious materials, 10-20 parts of organic matter, 0.6-1 parts of compound fertilizer, 0.08-0.1 parts of water retaining agent, and 20-30 parts of water are mixed and evenly mixed to form a vegetation matrix A, and the vegetation matrix A is filled into the gaps of the porous vegetation concrete by a high-pressure blowing method;
[0025] S3, attaching the vegetation matrix B to the surface of the vegetation porous concrete by dry spraying;
[0026] S4. Lay the infrared coconut fiber mesh on the porous vegetation concrete.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1. Traditional concrete materials have a dense structure and less iron oxide content inside the structure, which makes it difficult for electromagnetic waves to enter the material and has weak electromagnetic absorption capacity. The planted concrete of the present invention makes full use of the aperture structure of wine lees aggregates to enable it to absorb, reflect, scatter and interfere with electromagnetic waves, and enhances the electromagnetic absorption performance through iron salt modification, effectively improving the impedance matching characteristics and attenuation characteristics of concrete materials.
[0029] 2. The present invention adds the wave-absorbing distiller's grains biochar modified by iron salt as an admixture to the vegetation matrix A, so that it has the dual functions of absorbing waves and improving soil. On the one hand, the introduction of iron-based materials can increase the magnetism of biochar, so that the vegetation matrix has electromagnetic wave absorption function; on the other hand, the biochar itself has a porous structure, a large specific surface area and a strong cation exchange rate, which makes its adsorption capacity outstanding and helps to improve the soil's fertilizer retention capacity; in addition, the distiller's grains biochar prepared by the present invention has a low pH, which is beneficial to buffer the alkaline environment of concrete and is suitable for plant growth.
[0030] 3. The technology of using other bionic materials to simulate the unique spectral characteristics of plants to achieve visible light stealth has yet to be developed. However, the present invention helps the surface plants of the target project to change with the background season changes by optimizing and matching the planting seeds suitable for the natural succession law. In addition, the combination of perennial herbaceous plants and vines such as big Wufeng grass, ground ivy, wild sweet potato, etc. is conducive to increasing the green plant coverage area, reducing the contrast difference in brightness and chromaticity between the target project and the background, and has simple, economical and efficient visible light, infrared and radar stealth functions.
[0031] 4. Glass microbeads have good cooling and matting effects, and are light in weight and have good heat insulation performance. The infrared reflective pigment is close to the color of the plant, and has a high refractive index and high infrared reflectivity. The infrared reflective coating prepared by compounding the two materials has low reflection and high heat insulation, which can enhance the infrared stealth performance from two aspects. Coconut fiber net is a high-quality material to replace plastic three-dimensional net slope protection due to its excellent flexibility, environmental protection, impact resistance, corrosion resistance, moisture retention and heat preservation. The coconut fiber net coated with infrared reflective coating is laid on the surface of the vegetation concrete, which has the dual functions of matrix infrared stealth and slope protection and soil consolidation.
[0032] 5. The present invention recycles the lees residue in the form of lees pellets, lees plant fibers and lees powder by granulating lees, screening lees plant fibers and powder, and has high economic and ecological effects. On the one hand, lees powder is rich in nutrients such as amino acids, sugars, organic acids, proteins, etc., and its application in plant growth matrix has the effect of regulating soil acidity and alkalinity and enriching nutrition. On the other hand, the lees residue is rich in plant fibers, which can improve the structural stability of lees pellets and have wave absorbing properties after carbonization modification. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a schematic diagram of the structure of the present invention.
[0034] Figure 2 It is a test diagram of the visible light camouflage performance of Examples 1-4 of the present invention and the comparative example.
[0035] Figure 3 It is a test diagram of the infrared camouflage performance of Examples 1-4 of the present invention and the comparative example.
[0036] Figure 4 It is a test diagram of the electromagnetic camouflage performance of Examples 1-4 of the present invention and the comparative example. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] like Figure 1 As shown, the present invention provides a vegetation concrete structure for achieving multi-spectrum compatible camouflage, including porous vegetation concrete, a vegetation matrix A filled in the porous vegetation concrete, and a vegetation matrix B attached to the surface of the porous vegetation concrete, the porous vegetation concrete has an electromagnetic wave absorption function, the vegetation matrix A has electromagnetic wave absorption and soil improvement functions, plant seeds are mixed in the vegetation matrix B, and the plant seeds form vegetation coverage after growth, and the vegetation coverage has visible light and radar stealth functions.
[0039] In the embodiment of the present invention, the mixed cementitious material is a mixture of L-SAC 42.5 cement and PO 42.5 cement in a mass ratio of 1:1.
[0040] In an embodiment of the present invention, a method for preparing microwave-absorbing wine lees pellets comprises the following operations: placing wine lees waste residue with a moisture content of 25-30wt% after drying or pre-wetting treatment in a pelletizer to form wine lees pellets with a diameter of 1-1.5mm, and then placing the formed wine lees pellets in a muffle furnace under nitrogen conditions at 450°C for 4h, and modifying the wine lees pellets after pyrolysis by soaking in an iron salt solution to obtain the microwave-absorbing wine lees pellets.
[0041] In an embodiment of the present invention, the modification of the pyrolyzed distiller's grains by soaking them in an iron salt solution includes the following operations: soaking the pyrolyzed distiller's grains in an iron salt solution with a concentration of 1 mol / L for 12-24 hours, wherein the iron salt solution is one or more of FeSO4 solution, FeCl3 solution, Fe(NO4)2 solution, and Fe(Ac)2 solution; after the distiller's grains fully absorb the iron salt solution, they are removed and drained, placed in a muffle furnace and calcined at 400-450°C for 2 hours, and then washed with deionized water and dried after calcination.
[0042] In an embodiment of the present invention, the preparation method of wave-absorbing wine lees biochar includes the following operations: placing the wine lees residue in an oven at 90-100°C to dry, crushing it through a 16-18 mesh sieve, the part above the sieve is cereal plant fiber, and the part below the sieve is wine lees powder rich in amino acids, sugars, organic acids, and proteins, the sieved cereal plant fiber is subjected to oxygen-isolated high-temperature heating to obtain wine lees biochar, and then the wine lees biochar is soaked in an iron salt solution for modification to obtain the wave-absorbing wine lees biochar.
[0043] In an embodiment of the present invention, the sieved cereal plant fibers are subjected to oxygen-insulated high-temperature heating to obtain distiller's grain biochar, which includes the following operations: placing the cereal plant fibers in a muffle furnace for anaerobically pyrolysis at 450°C under nitrogen conditions for 2 hours, grinding them through an 80-100 mesh sieve to obtain biochar; the modification of the distiller's grain biochar by soaking it in an iron salt solution includes the following operations: mixing the distiller's grain biochar and the iron salt solution at a ratio of 100g / L and stirring them evenly for adsorption, the iron salt solution is one or more of FeSO4 solution, FeCl3 solution, Fe(NO4)2 solution, and Fe(Ac)2 solution, with a concentration of 1mol / L. After adsorption for 30 minutes, placing it in a muffle furnace and calcining it at 400-450°C for 2 hours, and washing and drying it with deionized water after calcination.
[0044] In an embodiment of the present invention, the preparation method of the infrared coconut fiber net is: prepare an infrared reflective coating from infrared reflective pigment, deionized water, additives, and glass beads, and then apply the infrared reflective coating to the coconut fiber net by spraying, brushing or rolling to obtain the infrared coconut fiber net.
[0045] In the embodiment of the present invention, the infrared reflective pigment is mixed with Cr2O3, Fe2O3, TiO2, and Al(OH)3 in a ratio of Cr:Fe:Ti:Al of 209.3:1:6.7:15.9, and then placed in a ball mill for wet mixing and grinding for 5 hours, taken out and centrifuged, dried, ground through a 200-mesh sieve, and then the sieve under the sieve is placed in a tubular atmosphere furnace, heated to 780-1080°C at a rate of 2°C / min and calcined for 3 hours to obtain the infrared reflective pigment;
[0046] The effective density of the glass microspheres is 0.32-0.40 g / cm 3, the average particle size is 30μm, and the particle size distribution is 16-60μm;
[0047] 10 parts of infrared reflective pigment, 30 parts of deionized water and 58 parts of auxiliary agents are prepared into color fillers in a certain proportion, wherein the auxiliary agents include 8 parts of kaolin, 24 parts of heavy calcium powder and 26 parts of AC-261P emulsion, and then glass beads are added in a proportion of 9-27% by mass of the color fillers to prepare infrared reflective coating.
[0048] Example 1
[0049] As a preferred embodiment of the present invention, the preparation method of the vegetation concrete structure of this embodiment includes the following steps:
[0050] S1. Forming 100 parts by weight of mixed cementitious materials, 630 parts by weight of absorbing wine lees pellets, 22 parts by weight of water, 10 parts by weight of water reducer, and 3 parts by weight of thickener into a vegetation porous concrete by using a pre-coating method;
[0051] S2, 7 parts by mass of absorbing wine lees biochar, 80 parts of soil, 15 parts of wine lees powder, 4 parts of mixed cementitious materials, 10 parts of organic matter, 0.8 parts of compound fertilizer, 0.09 parts of water retaining agent, and 20 parts of water are mixed and evenly mixed to form a vegetation matrix A, and the vegetation matrix A is filled into the gaps of the porous vegetation concrete by a high-pressure blowing method;
[0052] S3, 20% of annual herbs (ryegrass and cosmos), 35% of perennial herbs (big wufeng grass, reed fescue, lycopodium), 15% of vines (parthenocissus, wild sweet potato), 20% of perennial legumes (sainfoin, Medicago truncatula, Vicia glabra), 10% of perennial shrubs (Purple Sophora japonica, Pigeon pea, Sea buckthorn, Lespedeza) in percentage by mass are mixed evenly to obtain mixed planting seeds, and the planting matrix A is prepared according to S2 at 45 g / m 2 The amount of is mixed with the prepared vegetation matrix A to obtain the vegetation matrix B, and the vegetation matrix B is attached to the surface of the vegetation porous concrete by dry spraying;
[0053] S4. Lay the infrared coconut fiber mesh on the vegetation porous concrete. The amount of glass beads added to the infrared coconut fiber mesh is 9% of the color filler. The mesh size of the infrared coconut fiber mesh is 5*5cm, the wire diameter is 0.4-0.5cm, the strength is>0.8kN / m, and the tensile force it can withstand is ≥20kg.
[0054] Example 2
[0055] As a preferred embodiment of the present invention, the preparation method of the vegetation concrete structure of this embodiment includes the following steps:
[0056] S1. Forming 102 parts by weight of mixed cementitious materials, 650 parts by weight of lees pellets, 30 parts by weight of water, 11 parts by weight of water reducer, and 3 parts by weight of thickener into a vegetation porous concrete by a pre-coating method;
[0057] S2. 6 parts by mass of absorbing wine lees biochar, 78 parts by mass of soil, 12 parts by mass of wine lees powder, 5 parts by mass of mixed cementitious materials, 16 parts by mass of organic matter, 0.8 parts by mass of compound fertilizer, 0.09 parts by mass of water retaining agent, and 23 parts by mass of water are mixed and uniformly mixed to form a vegetation matrix A, and the vegetation matrix A is filled into the voids of the porous vegetation concrete by a high-pressure blowing method;
[0058] S3, 20% of annual herbaceous plants (Persian chrysanthemum), 35% of perennial herbaceous plants (Festuca australis, Elymus dahliae, Duckgrass, Bahia grass), 15% of vines (Parthenocissus, Ivy), 20% of perennial legumes (Sainfoin, Medicago truncatula, Vetch), 10% of perennial shrubs (Sophora japonica, Pigeon pea, Hippophae rhamnoides, Lespedeza bicolor) in percentage by mass are mixed evenly to obtain mixed planting seeds, and the planting matrix A is prepared according to S2 at a temperature of 35 g / m 2 The amount of is mixed with the prepared vegetation matrix A to obtain the vegetation matrix B, and the vegetation matrix B is attached to the surface of the vegetation porous concrete by dry spraying;
[0059] S4. Lay the infrared coconut fiber mesh on the vegetation porous concrete. The amount of glass beads added to the infrared coconut fiber mesh is 15% of the color filler. The mesh size of the infrared coconut fiber mesh is 5*5cm, the wire diameter is 0.4-0.5cm, the strength is>0.8kN / m, and the tensile force it can withstand is ≥20kg.
[0060] Example 3
[0061] As a preferred embodiment of the present invention, the preparation method of the vegetation concrete structure of this embodiment includes the following steps:
[0062] S1. 105 parts by weight of mixed cementitious materials, 660 parts by weight of lees pellets, 34 parts by weight of water, 11 parts by weight of water reducing agent, and 2 parts by weight of thickener are formed into a vegetation porous concrete by a pre-coating method;
[0063] S2, 7 parts by mass of absorbing wine lees biochar, 87 parts of soil, 13 parts of wine lees powder, 5 parts of mixed cementitious materials, 15 parts of organic matter, 0.9 parts of compound fertilizer, 0.09 parts of water retaining agent, and 25 parts of water are mixed and evenly mixed to form a vegetation matrix A, and the vegetation matrix A is filled into the gaps of the porous vegetation concrete by a high-pressure blowing method;
[0064] S3, 20% of annual herbaceous plants (ryegrass), 35% of perennial herbaceous plants (big wufeng grass, orchard grass, bahia grass), 15% of vines (ivy, wild sweet potato), 20% of perennial legumes (sainfoin, Medicago truncatula, Vicia glabra), 10% of perennial shrubs (Purple Sophora japonica, Pigeon pea, Sea buckthorn, Lespedeza) are mixed evenly to obtain mixed planting seeds, and the planting matrix A is prepared according to S2, at a rate of 50 g / m 2 The amount of is mixed with the prepared vegetation matrix A to obtain the vegetation matrix B, and the vegetation matrix B is attached to the surface of the vegetation porous concrete by dry spraying;
[0065] S4. Lay the infrared coconut fiber mesh on the vegetation porous concrete. The amount of glass beads added to the infrared coconut fiber mesh is 21% of the color filler. The mesh size of the infrared coconut fiber mesh is 5*5cm, the wire diameter is 0.4-0.5cm, the strength is>0.8kN / m, and the tensile force is ≥20kg.
[0066] Example 4
[0067] As a preferred embodiment of the present invention, the preparation method of the vegetation concrete structure of this embodiment includes the following steps:
[0068] S1. Forming 110 parts by weight of mixed cementitious materials, 670 parts by weight of absorbing wine lees pellets, 37 parts by weight of water, 11 parts by weight of water reducer, and 4 parts by weight of thickener into a vegetation porous concrete by a pre-coating method;
[0069] S2. Mix 6 parts of absorbing wine lees biochar, 90 parts of soil, 10 parts of wine lees powder, 6 parts of mixed cementitious materials, 10 parts of organic matter, 1 part of compound fertilizer, 0.1 parts of water retaining agent, and 30 parts of water by weight to make a vegetation matrix A, and fill the vegetation matrix A into the gaps of the porous vegetation concrete by high-pressure blowing method;
[0070] S3, 10% of annual herbaceous plants (ryegrass), 35% of perennial herbaceous plants (big wufeng grass, reed fescue, alkali grass, bahia grass), 10% of vines (parthenocissus, wild sweet potato, ivy), 20% of perennial legumes (sainfoin, Medicago truncatula, Vicia glabra), 10% of perennial shrubs (Purple Sophora japonica, Pigeon pea, Sea buckthorn, Lespedeza) are mixed evenly to obtain mixed planting seeds, and the planting matrix A is prepared according to S2 at 40 g / m 2 The amount of is mixed with the prepared vegetation matrix A to obtain the vegetation matrix B, and the vegetation matrix B is attached to the surface of the vegetation porous concrete by dry spraying;
[0071] S4. Lay the infrared coconut fiber mesh on the vegetation porous concrete. The amount of glass beads added to the infrared coconut fiber mesh is 27% of the color filler. The mesh size of the infrared coconut fiber mesh is 5*5cm, the wire diameter is 0.4-0.5cm, the strength is>0.8kN / m, and the tensile force is ≥20kg.
[0072] Comparative Example
[0073] In the bioreinforced concrete structure of this comparative example, the S1 absorbing wine grains pellets are replaced with ordinary wine grains pellets that have not been carbonized and modified by immersion in iron salt solution, no absorbing wine grains biochar and wine grains powder are added to S2, and the S4 mid-infrared coconut fiber mesh is replaced with ordinary coconut fiber mesh that is not coated with reflective coating. The rest is the same as Example 4.
[0074] Test Case
[0075] The performance of the vegetation concrete structure of each embodiment and comparative example was measured:
[0076] 1. pH determination: pH was determined using the potentiometric method (water-soil ratio of 2.5:1).
[0077] 2. Void ratio determination: refer to the "Permeable Concrete River Embankment Construction Manual" for determination, and the calculation formula is as follows:
[0078]
[0079] Where: P is the total porosity of the specimen (%); W1 is the weight of the specimen in water after immersion for 24 hours (g); W2 is the weight of the specimen in air after being taken out of water and left to stand naturally for 24 hours (g); V is the apparent volume of the specimen (m 3 ).
[0080] 3. Visible light camouflage performance test: Use plant cover to characterize the visible light camouflage effect (studies have shown that plant cover greater than 70% can achieve the purpose of visible light camouflage). Plant cover sampling needle puncture method measurement: Select a sample area of 1m*1m, with the help of a steel tape measure and marks every 2.5cm on the sample frame rope, use a thin needle about 2mm thick, and insert it vertically from the top of the vegetation in the sample at intervals of 62.5px up and down (a total of 100 points) in sequence. If the needle touches the plant, it is counted as a "yes", if there is no contact, it is counted as "no" and no mark is made. Finally, calculate the number of marks and express it as a percentage as the coverage.
[0081] 4. Infrared camouflage performance test: The infrared light heating experiment is used to test the infrared stealth performance of the infrared coconut silk net. An infrared bulb is selected as the radiation source. The light source is 30cm away from the sample surface. The light is incident vertically. The radiation intensity received by the sample surface is 1.88kW / m 2The infrared coconut fiber webs of Examples 1-4 and the comparative example were subjected to a heating experiment. The surface temperature of the samples was measured using a thermocouple.
[0082] 5. Electromagnetic camouflage performance test: The electromagnetic wave absorption performance test adopts the cross-section (RCS) method, which is the radar absorbing material reflectivity test method. The RCS method is used to measure the RAM reflectivity, and the measurement frequency range is 8GHz to 18GHz.
[0083] The performance test results are shown in Table 1. Figure 2 , Figure 3 , Figure 4 As shown:
[0084] Table 1
[0085] index Example 1 Example 2 Example 3 Example 4 Comparative Example 1 pH 7.60 7.57 8.01 7.52 9.02 Porosity (%) 33% 31% 32% 29% 28%
[0086] Vegetative concrete usually has a high pH due to the use of cementitious materials, and distiller's grains pellets and distiller's grains powder contain a large amount of organic acids, which have a regulating effect on the alkaline environment of the vegetation matrix. As can be seen from Table 1, in Examples 1-4 where distiller's grains pellets and distiller's grains powder were added, the alkaline environment was significantly improved, with a pH range of 7.52-8.01, while the pH of the comparative example without adding distiller's grains powder was as high as 9.02, which is not conducive to plant growth. In addition, the porosity of the vegetative concrete is required to be greater than 25%, and all the above implementation cases meet the requirements.
[0087] The plant coverage of vegetated concrete>70% can meet the camouflage requirements of the target substrate in the forest background. Figure 1 It can be seen that in Examples 1-4, the vegetation coverage is more than 70% after 60 days of plant growth, and Example 3 has the best vegetation recovery effect, with a coverage of 78% at 60 days and a coverage of 97% at 120 days. The vegetation recovery of the comparative example is slower, and it still has not reached 70% at 90 days, and only reaches 75% at 120 days. This shows that the present invention not only improves the vegetation coverage but also shortens the time for vegetation regreening, and can meet the coverage requirements of visible light camouflage in a short period of time (60 days), and the camouflage effect is better, which may be closely related to the pH of the examples meeting the vegetation requirements.
[0088] Depend on Figure 2 It can be seen that the infrared light heating rate of Examples 1-4 and the comparative example is: comparative example>Example 1>Example 4>Example 2>Example 3, that is, the coating of infrared reflective coating has a significant effect on reducing the infrared light heating rate of the coconut fiber mesh, among which Example 3 with the lowest temperature rise in 25 minutes is 12°C different from the comparative case. In addition, the glass beads content of Examples 1-4 are 9%, 15%, 21%, and 27%, respectively, among which Example 3 with a content of 21% shows the best effect of reducing the heating rate, indicating that there is no linear relationship between the heating rate and the glass beads content, and excessive addition may have a negative effect.
[0089] Depend on Figure 3 It can be seen that the addition of absorbing wine lees pellets and wine lees biochar has a significant effect on the electromagnetic reflectivity of the vegetation concrete. Example 3 improves the wave absorption performance of the ecological concrete in the 9.6-18 frequency band, improves the electromagnetic absorption band to 8.4GHZ, the absorption peak is at 15.45GHZ, and the reflectivity is -45.5dB; Example 2 improves the wave absorption performance of the ecological concrete in the 9.2-13.7 frequency band, and improves the electromagnetic absorption band to 4.5GHZ; Example 1 reduces the reflectivity of the vegetation concrete in the two frequency bands of 9.6-12.8GHZ and 15.9-18GHZ; Example 4 improves a narrower band of only 1.3-8.4GHZ.
[0090] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.
Claims
1. A vegetated concrete structure that realizes multi-spectrum compatible camouflage, characterized in that: It comprises a porous vegetation concrete with electromagnetic wave absorption function, a vegetation matrix A filled in the porous vegetation concrete with electromagnetic wave absorption and soil improvement function, a vegetation matrix B attached to the surface of the porous vegetation concrete, and an infrared coconut fiber net with infrared reflection function laid on the porous vegetation concrete, wherein plant seeds are mixed in the vegetation matrix B, and the plant seeds form a vegetation cover layer with visible light and radar stealth function after growth; The porous vegetation concrete comprises the following components by mass: 100-110 parts of mixed cementitious materials, 625-670 parts of wave-absorbing wine lees aggregates, 22-37 parts of water, 10-11 parts of water reducing agent, and 2-4 parts of thickener; The plant growth matrix A comprises the following components by mass: 6-8 parts of wave-absorbing wine lees biochar, 60-90 parts of soil, 10-20 parts of wine lees powder, 3-6 parts of mixed gelling materials, 10-20 parts of organic matter, 0.6-1 parts of compound fertilizer, 0.08-0.1 parts of water retaining agent, and 20-30 parts of water; The planting matrix B comprises a planting matrix A and mixed planting seeds mixed in the planting matrix A, wherein the mixed planting seeds in the planting matrix A are mixed in an amount of 25-50 g / m 2 ; The infrared coconut fiber net has a mesh size of 5*5cm, a wire diameter of 0.4-0.5cm, a strength of>0.8kN / m, and a tensile force of ≥20kg.
2. The vegetated concrete structure for achieving multi-spectrum compatible camouflage according to claim 1, characterized in that: The mixed cementitious material is prepared by mixing L-SAC 42.5 cement and PO 42.5 cement in a mass ratio of 1:
1.
3. The vegetated concrete structure for achieving multi-spectrum compatible camouflage according to claim 1, characterized in that: The preparation method of the wave-absorbing wine lees pellets comprises the following operations: placing wine lees waste residue with a moisture content of 25-30wt% after drying or pre-wetting treatment in a pelletizer to form wine lees pellets with a diameter of 1-1.5mm, then placing the formed wine lees pellets in a muffle furnace under nitrogen conditions at 450°C for 4h, and soaking the pyrolyzed wine lees pellets in an iron salt solution for modification to obtain the wave-absorbing wine lees pellets.
4. The vegetated concrete structure for achieving multi-spectrum compatible camouflage according to claim 3 is characterized in that: The modification of the pyrolyzed distiller's grains by soaking them in an iron salt solution comprises the following operations: soaking the pyrolyzed distiller's grains in an iron salt solution with a concentration of 1 mol / L for 12-24 hours, wherein the iron salt solution is one or more of FeSO4 solution, FeCl3 solution, Fe(NO4)2 solution, and Fe(Ac)2 solution; after the distiller's grains fully absorb the iron salt solution, they are removed and drained, placed in a muffle furnace and calcined at 400-450°C for 2 hours, and then washed with deionized water and dried after calcination.
5. The vegetated concrete structure for achieving multi-spectrum compatible camouflage according to claim 1 is characterized in that: The preparation method of the wave-absorbing vinasse biochar comprises the following operations: drying vinasse residue in an oven at 90-100° C., crushing through a 16-18 mesh sieve, wherein the portion above the sieve is grain plant fiber, and the portion below the sieve is the vinasse powder, heating the sieved grain plant fiber at high temperature in an oxygen-free manner to obtain vinasse biochar, and then modifying the vinasse biochar by soaking it in an iron salt solution to obtain the wave-absorbing vinasse biochar.
6. The vegetated concrete structure for achieving multi-spectrum compatible camouflage according to claim 5, characterized in that: The method of preparing distiller's grain biochar by high-temperature heating the sieved cereal plant fibers in oxygen isolation includes the following operations: placing the cereal plant fibers in a muffle furnace for anaerobic pyrolysis at 450°C under nitrogen conditions for 2 hours, grinding them through an 80-100 mesh sieve to obtain biochar; the method of modifying the distiller's grain biochar by soaking them in an iron salt solution includes the following operations: mixing the distiller's grain biochar and the iron salt solution at a ratio of 100g / L and stirring them evenly for adsorption, wherein the iron salt solution is one or more of FeSO4 solution, FeCl3 solution, Fe(NO4)2 solution, and Fe(Ac)2 solution, with a concentration of 1mol / L. After adsorption for 30 minutes, the mixture is placed in a muffle furnace and calcined at 400-450°C for 2 hours, and then washed with deionized water and dried after calcination.
7. The vegetated concrete structure for achieving multi-spectrum compatible camouflage according to claim 1 is characterized in that: The mixed vegetation seeds include the following components in mass percentage: 20% annual herbaceous plants, 35% perennial herbaceous plants, 15% vines, 20% perennial legumes, and 10% perennial shrubs. The annual herbaceous plants are one or more of ryegrass and cosmos, the perennial herbaceous plants are one or more of sedge, reed fescue, lycopersicon esculentum, orchard grass, and bahia grass, the vines are one or more of parthenocissus, wild sweet potato, and ivy, the perennial legumes are one or more of red clover, Medicago truncatula, and Vetch, and the perennial shrubs are one or more of Sophora japonica, Cajun pea, Hippophae rhamnoides, and Lespedeza bicolor.
8. The vegetated concrete structure for achieving multi-spectrum compatible camouflage according to claim 1 is characterized in that: The preparation method of the infrared coconut fiber net is as follows: infrared reflective paint is prepared from infrared reflective pigment, deionized water, additives and glass beads, and then the infrared reflective paint is applied to the coconut fiber net by spraying, brushing or rolling to obtain the infrared coconut fiber net.
9. The vegetated concrete structure for achieving multi-spectrum compatible camouflage according to claim 8, characterized in that: The infrared reflective pigment is prepared by mixing Cr2O3, Fe2O3, TiO2 and Al(OH)3 in a ratio of Cr:Fe:Ti:Al of 209.3:1:6.7:15.9, and then mixing in a ball mill and grinding for 5 hours. After taking out, centrifugation, drying and grinding through a 200-mesh sieve are performed, and then the sieve is placed in a tubular atmosphere furnace, heated to 780-1080°C at a speed of 2°C / min and calcined for 3 hours to obtain the infrared reflective pigment. The effective density of the glass microspheres is 0.32-0.40 g / cm 3 , the average particle size is 30μm, and the particle size distribution is 16-60μm; Infrared reflective pigment, deionized water and additives are prepared into pigments and fillers in proportion, and then glass beads are added in a proportion of 9-27% by mass of the pigments and fillers to prepare infrared reflective coating; preferably, the mass ratio of infrared reflective pigment, deionized water and additives is 10:30:58, and preferably, the additives include the following components in parts by mass: 8 parts of kaolin, 24 parts of heavy calcium powder and 26 parts of AC-261P emulsion.
10. A method for preparing a vegetated concrete structure that realizes multi-spectrum compatible camouflage according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Forming 100-110 parts by weight of mixed cementitious materials, 625-670 parts by weight of lees pellets, 22-37 parts by weight of water, 10-11 parts by weight of water reducing agent, and 2-4 parts by weight of thickener into a vegetation porous concrete by a pre-coating method; S2, 6-8 parts by mass of absorbing wine lees biochar, 60-90 parts of soil, 10-20 parts of wine lees powder, 3-6 parts of mixed cementitious materials, 10-20 parts of organic matter, 0.6-1 parts of compound fertilizer, 0.08-0.1 parts of water retaining agent, and 20-30 parts of water are mixed and evenly mixed to form a vegetation matrix A, and the vegetation matrix A is filled into the gaps of the porous vegetation concrete by a high-pressure blowing method; S3, using dry spraying method to attach the vegetation matrix B to the surface of the vegetation porous concrete; S4. Lay the infrared coconut fiber mesh on the porous vegetation concrete.
Citation Information
Patent Citations
Filled plant fiber, preparation method thereof, and high-strength plastic wave-absorbing concrete
CN111606616A
Recycled lightweight aggregate pervious concrete and preparation method thereof
CN112142393A