High-reflection composite disordered superstructure material and preparation method and application thereof

Through the double-layer composite disordered superstructure material, combined with Mie scattering theory and multiple scattering principle, scattering particle layers of different structural sizes are designed, which solves the problem of insufficient reflection bandwidth in the existing technology, and realizes broadband high reflection and high-efficiency radiant heat control , suitable for space refrigeration.

CN119019169AActive Publication Date: 2024-11-26SHANGHAI JIAOTONG UNIV

Patent Information

Application Number
CN202411104737.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-26
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The existing highly disordered scattering superstructure materials are difficult to expand the reflection bandwidth without increasing cost and complexity, especially in the infrared band, which limits their application in the field of space refrigeration.

Method used

Using a double-layer composite disordered superstructure material, the reflection efficiency of the 0.2-1μm and 1-8μm bands is regulated by designing scattering particle layers of different structural sizes, and combining Mie scattering theory and multiple scattering principle to achieve broadband high reflection.

Benefits of technology

It effectively expands the reflection bandwidth of the superstructure to 0.2~8μm, improves the spectral control capability and radiative thermal control performance, and maintains the advantages of low-cost and large-scale production, and is suitable for radiation refrigeration applications in different environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019169A_ABST
    Figure CN119019169A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of thermal control materials, and discloses a high-reflection composite disordered superstructure material and a preparation method and application thereof, and the material comprises a photo-thermal regulation superstructure composed of a long-wave reflection layer and a short-wave reflection layer which are highly disordered. The spatial distribution of scattering particles in the material is highly disordered, the appearance is white, the thickness is 200-1000 microns, the weighted average reflectivity of the solar spectrum band is 0.8-0.97, the regulation reflection band is 0.2-8 microns, the infrared emissivity is 0.75-0.92, and the material has the advantages of wide band, high reflection, simple construction, low cost, large scale and the like. The formed composite superstructure is easy to machine, and the applicability of the composite height disordered scattering type superstructure to special-shaped surfaces and bent surfaces is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of selective radiation thermal control materials, and in particular relates to a wide-band high-reflection composite disordered superstructure material and a preparation method and application thereof. Background Art

[0002] As global warming intensifies, summer temperatures continue to rise, and human demand for summer space cooling is also growing rapidly, causing the problem of energy consumption and carbon emissions around the world to become increasingly prominent. According to the International Energy Agency's statistical report, the global electricity consumption for building space cooling in 2016 was 2000TWh, equivalent to about 10% of the world's total electricity consumption in the same year; and according to the current development trend, by 2050, the global energy consumption for space cooling will increase to three times that of 2016, reaching 6200TWh. Based on considerations of environmental impact, radiant cooling, as a new space cooling method that does not require energy input and only uses the inherent characteristics of the surface material to achieve heat control of the covered object, has become a very potential solution.

[0003] The basic idea of ​​efficient space cooling or device cooling is to isolate the external solar radiation heat source while dissipating its own heat as much as possible. The efficiency of dissipating its own heat can be improved by selecting high reflectivity materials, but for broadband solar radiation whose energy distribution covers the ultraviolet band, visible band and even infrared band, how to achieve high reflection in the corresponding broadband becomes the key to determine efficient space cooling. At present, according to the different reflection spectral ranges, radiation cooling materials are generally divided into two types: narrow-band radiation cooling materials that concentrate on reflecting solar radiation in the 0.2-2.5μm band, and broadband radiation cooling materials that uniformly reflect the entire 0.2-8μm band. The former has high emissivity in the band greater than 2.5μm, while the latter has high emissivity only in the 8-13μm atmospheric window band.

[0004] As a new functional material design concept that integrates the dual advantages of high refractive index, low absorption coefficient and other intrinsic physical properties of materials with artificial configuration, superstructure has shown great application potential in spectral regulation and selective radiation. For example, the metal-based film combined with the patterned supersurface configuration proposed in Chinese patent CN112460836 A "Passive radiation cooling composite film" realizes the regulation of spectral performance in different bands, but this solution is limited by the intrinsic ultraviolet absorption characteristics of metals, and the reflectivity cannot be further improved. In addition, the high cost and scale problems of metal-based film preparation limit the promotion and application of this solution; for example, Chinese patent CN109343159A "A nonlinear laser limiting structure based on one-dimensional photonic crystal" forms a one-dimensional photonic crystal superstructure by stacking multiple layers of dielectrics. Although the photonic band gap can be controlled to achieve customized band photothermal performance control, the problems of too small thickness of each layer of dielectric and high preparation precision requirements also need to be solved.

[0005] In comparison, the scattering superstructure that uses highly disordered spatial distribution of scattering units to achieve broadband high reflectivity is extremely practical. By analyzing the coupling relationship between the target radiation wavelength, target bandwidth and the structural parameters of the scattering unit, the geometric shape, size, content and even spatial distribution of the scattering unit can be finely designed and controlled. When the site coordinates of the scattering unit in three-dimensional space, whose geometric shape and size match the target control band, conform to the Percus–Yevick hard sphere model, its spatial distribution is highly disordered. The photothermal control scattering superstructure constructed based on Mie scattering theory can achieve broadband high reflectivity. Since the reflection performance originates from the disorder of the distribution of scattering units with specific structural parameters in three-dimensional space, this form of superstructure has lower processing accuracy requirements. Combined with the selection of low-cost materials, the highly disordered scattering superstructure is expected to achieve low cost and scale without sacrificing performance.

[0006] Among the highly disordered scattering superstructures currently reported, single-layer structural coatings or films are generally the main ones. The single structural design limits the further expansion of the reflection band. This structural form often has poor reflection in the infrared band and can generally only achieve high reflection in the 0.2-2.5μm band. Therefore, under the premise of ensuring the low cost and large-scale production of highly disordered scattering superstructures, further expanding the superstructure form and preparing efficient radiation thermal control materials with a reflection bandwidth extending to the infrared band has very important engineering application background and research value. Summary of the invention

[0007] In order to solve the above problems, the present invention provides a high-reflection composite disordered superstructure material and its preparation method and application. The material has a wide-band high-reflection performance and is a superstructure composited by a highly disordered spatial structure.

[0008] The artificial design concept of scattering superstructures is reflected in the geometric structural parameters and spatial distribution form of the scattering unit. According to the coupling relationship between the target wavelength, bandwidth and structural parameters, the geometric shape and structural parameters of the scattering particles can be reasonably designed to match the strong scattering band with the target regulation band to produce the strongest spectral response; at the same time, when the distribution form of the above scattering particles in three-dimensional space conforms to the Percus-Yevick hard sphere model, the degree of disorder is high, and the scattering artificial superstructure constructed for the photothermal regulation target will achieve broadband high reflection targets based on Mie theory and multiple scattering principles. The existing publicly reported scattering superstructures are still mainly in the form of single-layer films or coatings. Although such a single form achieves efficient reflection in the ultraviolet and visible bands, it is difficult to effectively scatter the near-infrared and mid-infrared bands due to the structural parameter limitations of the scattering particles, which seriously limits the expansion of the reflection bandwidth. By using a double-layer composite highly disordered superstructure and designing structural parameters according to the scattering efficiency in different bands, the reflection bandwidth will be effectively broadened. While maintaining the original advantages of the disordered distribution scattering superstructure, a new idea of ​​selective radiation photothermal regulation can be introduced, thereby further promoting the practical application of the superstructure.

[0009] The technical solution of the present invention is as follows:

[0010] The present invention discloses a highly reflective composite disordered superstructure material, comprising a photothermal control superstructure consisting of two highly disordered long-wave reflection layers and a short-wave reflection layer, wherein the long-wave reflection layer is a bottom layer, the control band is 1 to 8 μm, and is made of scattering particles with an average structural size of 5 to 20 μm and a structural size distribution range of 3 to 50 μm; the short-wave reflection layer is a surface layer, the control band is 0.2 to 1 μm, and is made of scattering particles with an average structural size of 0.1 to 2 μm and a structural size distribution range of 0.02 to 5 μm.

[0011] The internal scattering particles of the superstructure material are highly disordered in spatial distribution, white in appearance, 200 to 1000 μm thick, with a weighted average reflectivity of 0.8 to 0.97 in the solar spectrum band, an infrared emissivity of 0.75 to 0.92, and a regulated reflection band of 0.2 to 8 μm.

[0012] The scattering particles are silicon oxide, yttrium oxide, magnesium aluminum spinel, zirconium oxide, zinc sulfide, aluminum oxynitride or yttrium aluminum garnet.

[0013] The present invention also discloses a method for preparing the above-mentioned high-reflection composite disordered superstructure material, which comprises the following steps:

[0014] (1) preparing two slurries of scattering particles of different structural sizes: dispersing dried scattering particles with an average structural size of 5 to 20 μm and a structural size distribution range of 3 to 50 μm and dried scattering particles with an average structural size of 0.1 to 2 μm and a structural size distribution range of 0.02 to 5 μm in a mixed solution of a dispersant and a binder, and then adding a defoaming agent and mixing, to prepare a scattering particle slurry of a large structural size and a scattering particle slurry of a small structural size;

[0015] (2) Forming the long-wave reflective layer: Casting the scattering particle slurry with a large structure size on the cast base film, curing it in situ at 10 to 40° C., and drying it for 3 to 24 hours to obtain a bottom layer as the long-wave reflective layer;

[0016] (3) Short-wave reflective layer forming: a scattering particle slurry with a small structure size is cast on the long-wave reflective layer for a second time, in-situ cured at 10 to 40° C., and dried for 1 to 24 hours to obtain a surface layer as a short-wave reflective layer;

[0017] (4) Preparation of composite disordered superstructure materials: After the composite disordered superstructure blank of the two highly disordered long-wave reflection layers and the short-wave reflection layers is dried and debonded, it is processed as required to obtain a material of a specific shape and / or size, and then sintered at a high temperature to obtain the composite disordered superstructure material.

[0018] Two structural sizes of the scattering particles are selected. In order to match the response to short-wave incident radiation, the structural size of small-sized scattering particles is preferably in the range of 0.1-2μm with an average particle size. In order to form a highly disordered spatial distribution superstructure and avoid the ordered spontaneous assembly of particles of similar sizes, the structural size distribution range of small-sized scattering particles is 0.02-5μm. In order to match the response to long-wave incident radiation, the structural size of large-sized scattering particles is preferably in the range of 5-20μm with an average particle size. In order to form a highly disordered spatial distribution superstructure and avoid the ordered spontaneous assembly of particles of similar sizes, the structural size distribution range of large-sized scattering particles is 3-50μm. Scattering particles of the two structural sizes are respectively used to prepare two uniform, stable, and disorderly dispersed ceramic slurries.

[0019] In one embodiment of the present invention, the total thickness of the long-wave reflection layer and the short-wave reflection layer after secondary casting is preferably 600-1400 μm. When the surface short-wave reflection layer is prepared by secondary casting, the scraper of the casting machine is 50-100 μm higher than the bottom long-wave reflection layer. The two layers of highly disordered reflective structures formed by scattering particles of specific sizes together constitute a composite photothermal regulation superstructure.

[0020] In one embodiment of the present invention, in step (4), the high temperature sintering temperature is preferably 700-1200° C., the sintering atmosphere is air or oxygen, and the sintering time is 2-8 hours.

[0021] In one embodiment of the present invention, in step (1), the dispersant is dispersed in distilled water, mixed and then a pre-prepared binder solution is added to obtain a mixed solution containing the dispersant and the binder.

[0022] In one embodiment of the present invention, the solvent of the binder solution is preferably distilled water, the amount of the binder solution added is 5 to 10 wt% of the slurry mass, and the solid content of the binder in the binder solution is 10 to 16 wt%; the binder is one or both of polyvinyl alcohol or polyvinyl butyral, which is used to in situ fix the spatial distribution of disordered scattering particles.

[0023] In one embodiment of the present invention, the scattering particles are preferably added in an amount of 75-85 wt % of the slurry mass.

[0024] In one embodiment of the present invention, the dispersant is preferably one or more of polyvinyl pyrrolidone, a copolymer of isobutylene and maleic anhydride, sodium dodecyl sulfate or polyethylene glycol, which is used to ensure that large and small scattering particles are evenly and disorderly distributed in the slurry; the amount of the dispersant added is 0.2 to 1.2 wt% of the mass of the scattering particles.

[0025] In one embodiment of the present invention, the defoaming agent is preferably one or more of n-propanol, isopropanol, n-butanol, isobutanol or tert-butanol; the amount of the defoaming agent added is 0.2-1 wt % of the mass of the scattering particles.

[0026] The present invention also discloses the application of the above-mentioned highly reflective composite disordered superstructure material as a radiation cooling substrate in a surface environment protected by the atmosphere or in a space environment without the protection of the atmosphere. The application of radiation cooling and heat control in a substrate facing solar radiation includes a surface building exterior wall, a surface building roof, an outer surface of a surface fixed or non-fixed facility, a space device shell, and a spacecraft skin.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The high-reflection composite disordered superstructure material of the present invention, by effectively combining two reflective layers with different structural parameters, regulates the two spectral ranges of 0.2-1μm and 1-8μm in bands, greatly expands the high-reflection band of the superstructure, and regulates the reflection band to 0.2-8μm. At the same time, on the basis of improving the spectrum regulation capability and radiation thermal control performance (solar reflectivity, mid-infrared emissivity) of the superstructure, it has the advantages of simple construction, low cost, and scalability. At the same time, due to the characteristics of the secondary casting in-situ curing molding technology, the composite superstructure after molding is easy to machine, ensuring the applicability of the composite highly disordered scattering superstructure to special-shaped surfaces and curved surfaces. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Schematic diagram of the structure of a wide-band high-reflection composite disordered superstructure material of the present invention, wherein 1 is a surface short-wave reflection layer composed of disorderly distributed scattering particles of small structural size, 2 is a bottom long-wave reflection layer composed of disorderly distributed scattering particles of large structural size, and 3 is the air medium in the gaps between the scattering particles;

[0030] Figure 2 This is a schematic diagram of a physical photograph of a high-reflective composite disordered superstructure material according to Example 1 of the present invention;

[0031] Figure 3 This is a schematic diagram of the microscopic cross-sectional structure of a high-reflective composite disordered superstructure material according to Example 3 of the present invention. DETAILED DESCRIPTION

[0032] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0033] Many specific details are set forth in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention, so the present invention is not limited to the specific implementation disclosed below.

[0034] A method for preparing a highly reflective composite disordered superstructure material of the present invention comprises the following steps:

[0035] (1) preparing two slurries of scattering particles of different structural sizes respectively: first, transferring scattering particles of structural size average particle size of 5-20 μm, structural size distribution range of 3-50 μm, and structural size average particle size of 0.1-2 μm into a vacuum drying oven for drying and standby; ultrasonically dispersing the dispersant in distilled water, stirring evenly, adding a certain amount of pre-prepared binder solution, continuing to stir until uniform, then adding the dried scattering particles, ultrasonically dispersing and stirring until mixed evenly, then adding an appropriate amount of defoaming agent, and stirring thoroughly until the slurry is stable and uniform, thereby preparing a slurry of scattering particles of large structural size; selecting scattering particles of structural size average particle size of 0.1-2 μm, structural size distribution range of 0.02-5 μm, and preparing a slurry of scattering particles of small structural size according to the above method;

[0036] (2) Forming the long-wave reflective layer: Casting the scattering particle slurry with a large structure size on the cast base film, curing it in situ at 10 to 40° C., and drying it for 3 to 24 hours to obtain a bottom layer as the long-wave reflective layer;

[0037] (3) Short-wave reflective layer forming: a scattering particle slurry with a small structure size is cast on the long-wave reflective layer for a second time, in-situ cured at 10 to 40° C., and dried for 1 to 24 hours to obtain a surface layer as a short-wave reflective layer;

[0038] (4) Preparation of composite disordered superstructure material: After the composite disordered superstructure blank of the two highly disordered long-wave reflection layer and the short-wave reflection layer is dried and debonded, it is processed as required to obtain a material of a specific shape and / or size, and then sintered at a high temperature to obtain a composite disordered superstructure material, the structural schematic diagram of which is shown in FIG. Figure 1 shown.

[0039] Example 1

[0040] A method for preparing a highly reflective composite disordered superstructure material according to embodiment 1 of the present invention comprises the following steps:

[0041] The scattering particles of the composite disordered superstructure material of this embodiment are zirconium oxide, the dispersant is a copolymer of isobutylene and maleic anhydride, the binder is a 12 wt % polyvinyl alcohol aqueous solution, and the defoaming agent is n-propanol.

[0042] (1) Two ceramic slurries of scattering particles of different structural sizes are prepared respectively: small-sized zirconium oxide particles with an average particle size of 0.5 μm and a distribution range of 0.2 to 1.5 μm are weighed and placed in a vacuum drying oven, dried at 50° C. for later use, so that the zirconium oxide scattering particles account for 75 wt% of the slurry mass; a copolymer of isobutylene and maleic anhydride as a dispersant is weighed, the mass of which is 0.5 wt% of the mass of the scattering particles, the dispersant is added into distilled water, and ultrasonically dispersed uniformly; a binder solution is weighed, the mass of which is 7 wt% of the mass of the scattering particles, added into distilled water mixed with the dispersant, ultrasonically stirred uniformly, and fully mixed; the dried scattering particles of small structural size are added into the above solution, ultrasonically dispersed, and stirred until the mixture is uniform; n-propanol is added as a defoaming agent, the mass of which is 4 wt% of the mass of the scattering particles, and further stirred fully until the slurry is stable and uniform, thereby obtaining a slurry of scattering particles of small structural size;

[0043] Weigh large-sized zirconium oxide particles with an average particle size of 8 μm and a distribution range of 3 to 15 μm, so that the zirconium oxide scattering particles account for 75 wt% of the slurry mass, and repeat the above slurry configuration process to obtain a scattering particle slurry with a large structural size.

[0044] (2) Forming of the long-wave reflective layer: A ceramic slurry prepared from large-sized zirconium oxide particles with an average particle size of 8 μm and a distribution range of 3 to 15 μm is cast on a cast film. The wet film thickness is controlled to be 1200 μm. The film is in-situ cured and dried at 30°C for 5 hours to obtain the bottom long-wave reflective layer.

[0045] (3) Forming of the short-wave reflective layer: A ceramic slurry prepared from small-sized zirconium oxide particles with an average particle size of 0.5 μm and a distribution range of 0.2 to 1.5 μm is cast on the long-wave reflective layer for a second time, and the total thickness of the cast wet film is controlled to be 1000 μm. The short-wave reflective layer is formed on the surface by in-situ curing and drying at 30°C for 2 hours.

[0046] (3) Preparation of composite disordered superstructure: After the composite disordered superstructure blank with the upper layer being the short-wave reflection layer and the lower layer being the long-wave reflection layer is completely dried and debonded at 55°C, it is mechanically cut into 45 mm × 25 mm blank pieces after post-processing, and then transferred to a high-temperature muffle furnace for sintering at 1300°C for 5 hours to obtain the broadband high-reflection composite disordered superstructure. The actual schematic diagram is shown in FIG. Figure 2 shown.

[0047] The wide-band high-reflection composite disordered superstructure prepared in this embodiment was measured with a thickness meter to have a thickness of 800 μm. The diffuse reflectance spectrum in the 0.2-8 μm band was tested by an ultraviolet-visible-near-infrared spectrophotometer and a Fourier transform infrared spectrometer. When the material prepared in this embodiment is used for substrate radiation cooling in a surface environment, the solar spectrum intensity absorbed by the atmosphere is used for calculation, and the weighted integral calculation is performed according to the AM1.5 standard solar spectrum intensity, and the weighted reflectance in the entire solar spectrum range is 0.96; the diffuse reflectance spectrum in the band above 8 μm is tested by a Fourier transform infrared spectrometer. Since this sample is a non-transmitting sample, the emissivity spectrum can be further calculated by "emissivity = 1-reflectivity", and then the infrared emissivity in the 8-13 μm band of the atmospheric window is calculated by weighted integral calculation according to the Planck blackbody radiation formula to be 0.82.

[0048] Example 2

[0049] A method for preparing a highly reflective composite disordered superstructure material according to embodiment 2 of the present invention comprises the following steps:

[0050] The scattering particles involved in the composite disordered superstructure of this embodiment are magnesium aluminum spinel particles, the dispersant is sodium dodecyl sulfate, the binder is a 16 wt % polyvinyl alcohol aqueous solution, and the defoaming agent is n-butanol.

[0051] (1) Two ceramic slurries of scattering particles of different structural sizes are prepared respectively: small-sized magnesium-aluminum spinel particles with an average particle size of 0.3 μm and a distribution range of 0.1 to 1 μm are weighed and placed in a vacuum drying oven, dried at 50° C. for later use, so that the magnesium-aluminum spinel particles account for 80 wt% of the slurry mass; sodium dodecyl sulfate as a dispersant is weighed, the mass of which is 0.8 wt% of the mass of the scattering particles, and the dispersant is added into distilled water, and ultrasonically dispersed uniformly; a binder solution is weighed, the mass of which is 10 wt% of the mass of the scattering particles, and is added into distilled water mixed with the dispersant, and ultrasonically stirred uniformly and fully mixed; the dried scattering particles of small structural size are added into the above solution, and ultrasonically dispersed and stirred until the mixture is uniform; n-butanol is added as a defoaming agent, the mass of which is 4 wt% of the mass of the scattering particles, and further stirred fully until the slurry is stable and uniform, thereby obtaining a slurry of scattering particles of small structural size;

[0052] Weigh large-sized magnesium-aluminum spinel particles with an average particle size of 15 μm and a distribution range of 5 to 25 μm, so that the magnesium-aluminum spinel scattering particles account for 80 wt% of the slurry mass, repeat the above slurry configuration process to obtain a scattering particle slurry with a large structural size.

[0053] (2) Forming of the long-wave reflective layer: A ceramic slurry prepared from large-sized magnesium-aluminum spinel particles with an average particle size of 15 μm and a distribution range of 5 to 25 μm is cast on a cast film. The wet film thickness is controlled to be 1000 μm. The film is in-situ cured and dried at 20°C for 10 hours to obtain the bottom long-wave reflective layer.

[0054] (3) Forming of the short-wave reflective layer: A ceramic slurry prepared from small-sized magnesium-aluminum spinel particles with an average particle size of 0.3 μm and a distribution range of 0.1 to 1 μm is cast on the long-wave reflective layer for a second time, and the total thickness of the cast wet film is controlled to be 900 μm. The short-wave reflective layer is formed on the surface by in-situ curing and drying at 20°C for 4 hours.

[0055] (4) Preparation of composite disordered superstructure: After the composite disordered superstructure blank with the upper layer being the short-wave reflection layer and the lower layer being the long-wave reflection layer is completely dried and debonded at 60°C, it is mechanically cut into 40 mm × 40 mm blank sheets and then transferred to a high-temperature muffle furnace for sintering at 1000°C for 4 hours to obtain the wide-band high-reflection composite disordered superstructure.

[0056] The wide-band high-reflection composite disordered superstructure prepared in this embodiment was measured with a thickness meter to have a thickness of 730 μm. The diffuse reflectance spectrum of the 0.2-8 μm band was tested by an ultraviolet-visible-near-infrared spectrophotometer and a Fourier transform infrared spectrometer. When the material prepared in this embodiment is used for substrate radiation cooling in a space environment, the solar radiation energy is not attenuated due to the loss of atmospheric protection. Therefore, the weighted integral calculation is performed according to the AM0 standard solar spectrum intensity, and the solar weighted reflectance is 0.94. The diffuse reflectance spectrum of the band above 8 μm is tested by a Fourier transform infrared spectrometer. Since this sample is a non-transmitting sample, the emissivity spectrum can be further calculated by "emissivity = 1-reflectivity". Similarly, since there is no atmospheric protection, the calculation is no longer performed only for the 8-13 μm band. According to the Planck blackbody radiation formula, the blackbody radiation intensity at a temperature of 300K is calculated, and the infrared emissivity of the band greater than 8 μm is calculated by weighted integral calculation to be 0.88.

[0057] Example 3

[0058] A method for preparing a high-reflective composite disordered superstructure material according to embodiment 3 of the present invention comprises the following steps:

[0059] The scattering particles involved in the composite disordered superstructure of this embodiment are yttrium oxide particles, the dispersant is a copolymer of isobutylene and maleic anhydride, the binder is a 14 wt % polyvinyl alcohol aqueous solution, and the defoaming agent is n-propanol.

[0060] (1) Two ceramic slurries of scattering particles of different structural sizes are prepared respectively: small-sized yttrium oxide particles with an average particle size of 0.4 μm and a distribution range of 0.1 to 1.2 μm are weighed and placed in a vacuum drying oven, dried at 50° C. for later use, so that the yttrium oxide scattering particles account for 78 wt% of the slurry mass; a dispersant copolymer of isobutylene and maleic anhydride is weighed, the mass of which is 0.3 wt% of the mass of the scattering particles, and the dispersant is added to distilled water, and ultrasonically dispersed uniformly; a binder solution is weighed, the mass of which is 10 wt% of the mass of the scattering particles, and is added to distilled water mixed with the dispersant, ultrasonically stirred uniformly, and fully mixed; the dried scattering particles of small structural size are added to the above solution, ultrasonically dispersed, and stirred until the mixture is uniform; n-propanol is added as a defoaming agent, the mass of which is 4 wt% of the mass of the scattering particles, and further stirred fully until the slurry is stable and uniform, thereby obtaining a slurry of scattering particles of small structural size;

[0061] Weigh large-sized yttrium oxide particles with an average particle size of 29 μm and a distribution range of 10 to 45 μm, so that the yttrium oxide scattering particles account for 75 wt% of the slurry mass, repeat the above slurry configuration process to obtain a scattering particle slurry with a large structural size.

[0062] (2) Forming of the long-wave reflective layer: A ceramic slurry prepared from large-sized yttrium oxide particles with an average particle size of 29 μm and a distribution range of 10 to 45 μm is cast on a cast film. The wet film thickness is controlled to be 900 μm. The film is in-situ cured and dried at 30°C for 6 hours to obtain the bottom long-wave reflective layer.

[0063] (3) Forming of the short-wave reflective layer: A ceramic slurry prepared from small-sized yttrium oxide particles with an average particle size of 0.4 μm and a distribution range of 0.1 to 1.2 μm is cast on the long-wave reflective layer for a second time, and the total thickness of the cast wet film is controlled to be 800 μm. The short-wave reflective layer is formed on the surface by in-situ curing and drying at 30°C for 2 hours.

[0064] (4) Preparation of composite disordered superstructure: After the composite disordered superstructure blank with the upper layer being the short-wave reflection layer and the lower layer being the long-wave reflection layer is completely dried and debonded at 60°C, it is mechanically cut into 40 mm × 40 mm blank pieces after post-processing, and then transferred to a high-temperature muffle furnace for sintering at 1050°C for 6 hours to obtain the broadband high-reflection composite disordered superstructure. The schematic diagram of its microscopic cross-sectional structure is shown in FIG. Figure 3 As shown, the double-layer composite structure can be clearly seen.

[0065] The wide-band high-reflection composite disordered superstructure prepared in this embodiment was measured with a thickness meter to have a thickness of 550 μm. The diffuse reflectance spectrum in the 0.2-8 μm band was tested by an ultraviolet-visible-near-infrared spectrophotometer and a Fourier transform infrared spectrometer. When the material prepared in this embodiment is used for substrate radiation cooling in a surface environment, the solar spectrum intensity absorbed by the atmosphere is used for calculation, and the weighted integral calculation is performed according to the AM1.5 standard solar spectrum intensity, and the weighted reflectance in the entire solar spectrum range is 0.95; the diffuse reflectance spectrum in the band above 8 μm is tested by a Fourier transform infrared spectrometer. Since this sample is a non-transmitting sample, the emissivity spectrum can be further calculated by "emissivity = 1-reflectivity", and then the infrared emissivity in the 8-13 μm band of the atmospheric window is calculated by weighted integral calculation according to the Planck blackbody radiation formula to be 0.84.

[0066] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A highly reflective composite disordered superstructure material, It is characterized in that The invention comprises a photothermal regulation superstructure composed of two highly disordered long-wave reflection layers and a short-wave reflection layer, wherein the long-wave reflection layer is the bottom layer, the regulation band is 1-8 μm, and it is made of scattering particles with an average structure size of 5-20 μm and a structure size distribution range of 3-50 μm; the short-wave reflection layer is the surface layer, the regulation band is 0.2-1 μm, and it is made of scattering particles with an average structure size of 0.1-2 μm and a structure size distribution range of 0.02-5 μm. The internal scattering particles of the superstructure material are highly disordered in spatial distribution, white in appearance, 200 to 1000 μm thick, with a weighted average reflectivity of 0.8 to 0.97 in the solar spectrum band, an infrared emissivity of 0.75 to 0.92, and a regulated reflection band of 0.2 to 8 μm. The scattering particles are silicon oxide, yttrium oxide, magnesium aluminum spinel, zirconium oxide, zinc sulfide, aluminum oxynitride or yttrium aluminum garnet.

2. A method for preparing the highly reflective composite disordered superstructure material as claimed in claim 1, It is characterized in that The method comprises the following steps: (1) preparing two slurries of scattering particles of different structural sizes: dispersing dried scattering particles with an average structural size of 5 to 20 μm and a structural size distribution range of 3 to 50 μm and dried scattering particles with an average structural size of 0.1 to 2 μm and a structural size distribution range of 0.02 to 5 μm in a mixed solution of a dispersant and a binder, and then adding a defoaming agent and mixing, to prepare a scattering particle slurry of a large structural size and a scattering particle slurry of a small structural size; (2) Forming the long-wave reflective layer: Casting the scattering particle slurry with a large structure size on the cast base film, curing it in situ at 10 to 40° C., and drying it for 3 to 24 hours to obtain a bottom layer as the long-wave reflective layer; (3) Short-wave reflective layer forming: a scattering particle slurry with a small structure size is cast on the long-wave reflective layer for a second time, in-situ cured at 10 to 40° C., and dried for 1 to 24 hours to obtain a surface layer as a short-wave reflective layer; (4) Preparation of composite disordered superstructure material: After the two highly disordered long-wave reflection layers and short-wave reflection layers are dried and debonded, they are sintered at high temperature to obtain the composite disordered superstructure material.

3. The method for preparing the highly reflective composite disordered superstructure material according to claim 2, It is characterized in that The total thickness of the long-wave reflection layer and the short-wave reflection layer after secondary casting is 600-1400 μm. When the surface short-wave reflection layer is prepared by secondary casting, the scraper of the casting machine is 50-100 μm higher than the bottom long-wave reflection layer.

4. The method for preparing the highly reflective composite disordered superstructure material according to claim 2, It is characterized in that In step (4), the high temperature sintering temperature is 700-1200° C., the sintering atmosphere is air or oxygen, and the sintering time is 2-8 hours.

5. The method for preparing the highly reflective composite disordered superstructure material according to claim 2, It is characterized in that In step (1), the dispersant is dispersed in distilled water, mixed and then the pre-prepared binder solution is added to obtain a mixed solution containing the dispersant and the binder.

6. The method for preparing the highly reflective composite disordered superstructure material according to claim 5, It is characterized in that The solvent of the binder solution is distilled water, the amount of the binder solution added is 5-10wt% of the slurry mass, the solid content of the binder in the binder solution is 10-16wt%; the binder is one or both of polyvinyl alcohol and polyvinyl butyral.

7. The method for preparing the highly reflective composite disordered superstructure material according to claim 2, It is characterized in that The added amount of the scattering particles is 75-85wt% of the slurry mass.

8. The method for preparing the highly reflective composite disordered superstructure material according to claim 2, It is characterized in that The dispersant is one or more of polyvinyl pyrrolidone, copolymer of isobutylene and maleic anhydride, sodium dodecyl sulfonate or polyethylene glycol; the added amount of the dispersant is 0.2-1.2wt% of the mass of the scattering particles.

9. The method for preparing the highly reflective composite disordered superstructure material according to claim 2, It is characterized in that The defoaming agent is one or more of n-propanol, isopropanol, n-butanol, isobutanol or tert-butanol; The added amount of the defoamer is 0.2-1wt% of the mass of the scattering particles.

10. Use of the highly reflective composite disordered superstructure material according to claim 1 as a radiation cooling substrate in a surface environment protected by the atmosphere or in a space environment without the atmosphere.

Citation Information

Patent Citations

  • Sintered compact for wavelength conversion

    CN104900786A

  • Radiative cooling structures and systems

    CN109070695A

  • Composite radiation refrigeration film, composite radiation refrigeration film material and application thereof

    CN110972467A

  • Composite cooling film and article including same

    CN113874213A

  • MgO coating for radiation cooling and preparation process thereof

    CN115651460A

Cited By