Cyclic imide derivative, hydrothermal synthesis method thereof and application of cyclic imide derivative in flow battery
Through the hydrothermal synthesis method of imide derivatives, the water solubility and conjugation of molecules are increased, and the problems of low conjugation of anode electrolyte molecules and low dual electron storage stability in liquid flow batteries are solved, achieving high efficiency The dual electron transfer and stable electrochemical properties are suitable for commercial large-scale energy storage applications.
Patent Information
- Application Number
- CN202411123045.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-15
AI Technical Summary
In existing flow batteries, the anode electrolyte molecules are low in conjugation, the dual electron storage stability is not high, and the traditional synthesis method of imide derivatives is high cost and long time, which limits its application in neutral water flow batteries. .
Using an imide derivative and its hydrothermal synthesis method, the water solubility and conjugation of molecules are increased by ionized dimethylammonium and other water-soluble modifications, and a two-step reaction is used to simplify the synthesis process and avoid expensive use. organic solvent.
It realizes high conjugation and stable dual electron transfer of imide molecules, improves the dual electron storage stability and electrochemical performance of the flow battery, reduces the synthesis cost and time, and is suitable for low-cost, high-capacity, and large Power neutral water-based organic liquid flow battery.
Smart Images

Figure CN119019411A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrolyte materials for liquid flow batteries, and in particular relates to a class of cyclic imide derivatives and a hydrothermal synthesis method thereof and application thereof in liquid flow batteries. Background Art
[0002] Energy is an important material basis of the national economy. Its development and effective utilization are directly related to the level of production technology and living standards. With the rapid development of renewable energy, how to effectively store and regulate these volatile energy sources has become an important issue. Therefore, we urgently need to develop new and efficient large-scale energy storage technologies. Large-scale energy storage technology needs to meet at least three conditions: high safety, economy and green environmental protection. Traditional large-scale energy storage technologies are mainly divided into three categories: physical energy storage, battery energy storage and electrochemical energy storage. However, these energy storage technologies cannot meet power and capacity at the same time. Liquid flow battery is a high-performance battery that uses positive and negative electrolytes to separate and circulate separately. It has the characteristics of high capacity, wide application field and long cycle life. Its working principle is to achieve the mutual conversion of electrical energy and chemical energy through the reversible redox reaction of the active substances in the positive and negative electrolyte solutions. This feature makes liquid flow batteries play an important role in energy storage and regulation. According to the active substances, they can be divided into inorganic and organic liquid flow batteries. Inorganic liquid flow batteries mainly include vanadium-based, zinc-based and iron-based. Organic flow batteries can be divided into aqueous, non-aqueous and hybrid organic flow batteries. Aqueous flow batteries can be classified into acidic, alkaline and neutral aqueous flow batteries according to pH. Transition metal flow batteries have low energy density, high toxicity, special ion exchange membranes, high costs, potential environmental problems, etc. Aqueous RFBs have great potential in the field of energy storage due to their flexibility, stability, scalability, adjustability and safety.
[0003] As a key part of flow batteries, electrolyte materials play a vital role in the capacity and stability of batteries. The development of low-cost, environmentally friendly and highly stable positive and negative electrolytes is a difficult problem that needs to be solved. Although viologen and its derivative molecules are widely used in flow batteries, the traditional viologen electrolyte materials have a low degree of conjugation. In the process from the oxidized state to the highly reduced state, the pyridine ring changes from aromatic to antiaromatic, which seriously affects the stability of the two electrons. Therefore, generally speaking, viologen and its derivatives are mostly used for single electron storage.
[0004] Recently, imide substances have also begun to be used in liquid flow batteries. For example, after gaining electrons, the aromaticity of imide derivatives is enhanced, which is beneficial to the stability of the two electrons. However, the traditional synthesis method is not only costly, but also wastes time, labor and other energy, which hinders its commercial development. Therefore, it is urgent to find new synthesis methods to reduce costs. Accessing imide molecules is of great significance for the development of commercial neutral aqueous flow batteries using naphthylimide molecules. Summary of the invention
[0005] In view of the technical problems that the existing anode electrolyte molecules have low conjugation and low two-electron storage stability, and the long synthesis time and high cost of existing imide derivatives limit their commercial development and application in neutral aqueous flow batteries, the present invention aims to provide a class of imide derivatives and their hydrothermal synthesis method and application.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides an imide derivative, wherein the imide derivative is any one of the following structural formulas:
[0008]
[0009] Among them, R1 is Any one of the groups;
[0010] R2 is Any one of the groups;
[0011] n is 1 or 2.
[0012] A method for preparing the above-mentioned imide derivative comprises:
[0013] S1, preparation of precursor B;
[0014] S2, the precursor B of step S1 reacts with Cl-R2 to obtain a reaction solution, precipitates and filters, and dries to obtain an imide derivative;
[0015] The preparation of precursor B comprises: dissolving precursor A, adding Reaction to obtain precursor B;
[0016] The precursor A is any one of the following structural formulas
[0017]
[0018] Said In the example, R1 is Any one of the groups;
[0019] n is 1 or 2.
[0020] The precursor A and The molar ratio is 1:3.
[0021] The solvent for dissolving the precursor A is any one of toluene, N,N-dimethylformamide and tetrahydrofuran.
[0022] The molar ratio of the precursor B to Cl-R2 is 1:3;
[0023] In the Cl-R2, R2 is Any one of the groups.
[0024] The S2 reaction temperature is 110° C. to 130° C., and the reaction time is 22 h to 26 h.
[0025] The S2 precipitate was prepared by sequentially adding ethanol and acetone according to a volume ratio of 1:10:2 of reaction solution: ethanol: acetone.
[0026] The preparation of the precursor B is carried out at 110° C. to 130° C. for 20 h to 26 h.
[0027] The above-mentioned type of imide derivative is used in a liquid flow battery, wherein the liquid flow battery uses the imide derivative as the anode electrolyte and the MiAcNH-TEMPO solution as the cathode electrolyte.
[0028] The volume ratio of the anolyte to the cathode electrolyte is 1:2.5-3.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The invention discloses an imide derivative, which increases the water solubility of molecules by ionizing dimethylammonium and modifying other water solubilities. The water-soluble groups are increased from two to four or more, which not only increases the water solubility of the molecules, but also increases the molecular size as the water-soluble groups increase. Compared with viologen molecules, the imide molecules of the invention have stronger conjugation and aromaticity and larger molecular volume. The conjugation gradually increases from pyromellitic acid diimide to naphthalene diimide and then to perylene diimide. The strong conjugation makes the band gap of the imide molecules narrower, and can realize rapid electron transfer, thereby realizing stable double electron transfer. The invention solves the technical problems that the existing anode electrolyte molecules (such as viologen) have weak conjugation and low double electron storage stability.
[0031] The hydrothermal synthesis method of the imide derivative disclosed by the invention can be realized by only two steps of reaction, and the reaction time is shortened. The terminal N atom is ionized and modified to introduce multiple hydrophilic groups, thereby expanding the molecular size and improving the water solubility of the molecule. Compared with the imide molecules of the traditional synthesis method whose side chains are quaternary ammonium salts, hydroxyls, phosphates or sulfonates, the use of organic solvents such as N,N-dimethylformamide, tetrahydrofuran and acetonitrile can be effectively avoided, the solvent used in the reaction is low in price, the method is simple, the yield is high, and a large amount of synthesis is possible.
[0032] The present invention discloses an application of an imide derivative as a negative electrode electrolyte in a liquid flow battery. The negative electrode electrolyte is prepared by using a class of imide derivatives of the present invention, ionized TEMPO is used as a positive electrode electrolyte, and a DSVN membrane is used as an anion exchange membrane to form a neutral aqueous organic liquid flow battery with double electron storage. The imide derivatives of the present invention have high solubility in water, a large output voltage within the range of water electrolysis, a relatively negative redox potential, and a reversible redox peak, and exhibit extremely strong double electron stability in electrochemical tests. The imide derivatives of the present invention can be used for low-cost, high-capacity, high-power, and long-life neutral aqueous organic liquid flow batteries, which are suitable for commercial large-scale energy storage and are of great significance to the development of imide derivatives in neutral aqueous liquid flow batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is a CV curve diagram of the imide derivative Pry-NDI of the present invention;
[0034] Figure 2 It is a full-cell CV curve diagram of a battery assembled with the imide derivative Pry-NDI of the present invention;
[0035] Figure 3 This is an electrochemical test diagram of a battery assembled with the imide derivative Pry-NDI of the present invention;
[0036] Figure 4 This is an electrochemical test diagram of a battery assembled with the imide derivative diol-PyrNDI of the present invention. DETAILED DESCRIPTION
[0037] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0038] Example 1 Synthesis of Imidyl Derivative Pry-NDI
[0039] Take n = 2, R1 is R2 is
[0040] Precursor A is
[0041] (1) Preparation of precursor B:
[0042] The chemical reaction equation of precursor B is:
[0043]
[0044] In a reaction kettle, 15 g of precursor A was dissolved in 100 mL of toluene, 17.15 g of 1-(3-aminopropyl)pyrrole was added, and the mixture was heated to 120° C. for 24 h. After the reaction was completed, the mixture was filtered, and the golden solid was washed with ethanol three times and then vacuum dried to obtain precursor B. The structural formula of precursor B is as follows:
[0045]
[0046] (2) Synthesis of imide derivative Pry-NDI
[0047] In a high-pressure reactor, weigh 10 g of precursor B and 6.63 g of Cl-CH3 and place them in 59.8 mL of 1 mol L -1 The reaction mixture was added to a tetrahydrofuran solution at 120° C. for 24 hours to obtain a reaction solution; ethanol and acetone were added in sequence at a volume ratio of 1:10:2 reaction solution: ethanol: acetone. After the solid precipitated, it was filtered, washed with acetone three times, and dried in vacuo to obtain a light yellow powder of the imide derivative Pry-NDI with a yield of 90%.
[0048] The structural formula of the obtained imide derivative Pry-NDI is shown below:
[0049]
[0050] The specific hydrogen spectrum data of the obtained imide derivative Pry-NDI are as follows:
[0051] 1 H NMR (400MHz, Deuterium Oxide) δ8.62 (s, 4H), 4.23 (t, J = 7.0Hz, 4H), 3.60–3.47 (m, 12H), 3.04 (s, 6H), 2.31–2.16 (m, 12H).
[0052] It is proved that the above process synthesizes the compound.
[0053] Example 2: Synthesis of imide derivative Pyrdiol-NDI
[0054] Take n = 2, R1 is R2 is
[0055] Precursor A is
[0056] (1) Preparation of precursor B:
[0057] The chemical reaction equation of precursor B is:
[0058]
[0059] In a reaction kettle, 15 g of precursor A was dissolved in 100 mL of N,N-dimethylformamide, 17.15 g of N-(3-aminopropyl)pyrrole was added, and the mixture was heated to 120°C for 24 h. After the reaction, the mixture was filtered, and the golden yellow powder was washed with ethanol three times and then vacuum dried to obtain precursor B. The structural formula of precursor B is as follows:
[0060]
[0061] (2) Synthesis of imide derivative Pry-NDI:
[0062] In a high-pressure reactor, 10 g of the precursor B obtained in (1) and 6.63 g of Cl-R2 were weighed and placed in 10 mL of water. The mixture was reacted at 120° C. for 24 h to obtain a reaction solution. Ethanol and acetone were added in sequence at a volume ratio of 1:10:2 of reaction solution: ethanol: acetone. After the solid precipitated, it was filtered, washed with acetone three times, and dried in vacuo to obtain a yellow powder of the imide derivative Pyr-diolNDI with a yield of 93%.
[0063] The structural formula of the obtained imide derivative Pyr-diolNDI is shown below:
[0064]
[0065] The specific hydrogen spectrum data of the obtained imide derivative Pry-diolNDI are as follows:
[0066] 1 H NMR (400MHz, Deuterium Oxide) δ8.61 (s, 4H), 4.28–4.11 (m, 6H), 3.69–3.36 (m, 20H), 2.19 (s, 12H).
[0067] Example 3: Synthesis of imide derivative dex-MoTPDI
[0068] Take n = 2, R1 is R2 is
[0069] Precursor A is
[0070] (1) Preparation of Precursor B
[0071] The reaction formula of precursor B is as follows:
[0072]
[0073] In a reaction kettle, 10 g of compound A was dissolved in 100 mL of toluene, 11.03 g of 1-(3-aminopropyl)morpholine was added, and the mixture was heated to 120° C. for 24 h. After the reaction was completed, the mixture was filtered, and the brown solid was washed with ethanol three times and then vacuum dried to obtain precursor B. The structural formula of precursor B is as follows:
[0074]
[0075] (2) Synthesis of imide derivative dex-MoTPDI
[0076] In a high-pressure reactor, 10 g of precursor B and 8.78 g of 3-chloro-2-hydroxypropyltrimethylammonium chloride were weighed and placed in 15 mL of water, and the reaction was carried out at 120° C. for 24 h to obtain a reaction solution; ethanol and acetone were added in sequence at a volume ratio of 1:10:2 product: ethanol: acetone, and solids were precipitated and filtered, washed with acetone 3 times, and dried in vacuo to obtain a red powder of the imide derivative dex-TPDI with a yield of 85%.
[0077] The structural formula of dex-MoTPDI is shown below:
[0078]
[0079] Example 4: Application of the imide derivatives of the present invention as anode electrolyte materials
[0080] The neutral aqueous organic flow battery electrode material is prepared by using the imide derivative Pyr-NDI prepared in Example 1 and Example 2, which can be prepared by the following steps:
[0081] Step 1: Assemble the core fixture
[0082] The neutral aqueous organic redox flow battery used in the test is a single cell structure. The positive terminal plate, positive insulating plate, positive conductive plate, positive flow frame, positive graphite felt, positive gasket, anion exchange membrane, negative gasket, negative graphite felt, negative flow frame, negative conductive plate, negative insulating plate, and negative terminal plate are fixed with bolts in turn, and external pipes are connected. Check whether the bolts are loose. If they are loose, they can be reinforced again. Before the test, a sealing and pressure test should be performed. On the basis of the above-mentioned fixture, two liquid storage bottles and a peristaltic pump are connected. After 2 hours of circulation, if there is no leakage and no change in liquid volume, it can be retained for use. If the above-mentioned leaks occur, readjustment is required.
[0083] Step 2: Preparation of electrode materials
[0084] Prepare a sufficient amount of 2M NaCl solution in a volumetric flask. The cathode electrolyte uses a methylimidazole-functionalized (2,2,6,6-tetramethylpiperidin-1-yl)oxy solution with the chemical formula C 15 H 26 N4O2, referred to as MiAcNH-TEMPO.
[0085] (1) Preparation of 0.1M Pry-NDI / 0.1M MiAcNH-TEMPO neutral aqueous organic flow battery
[0086] Take 362mg Pry-NDI and 495mg MiAcNH-TEMPO and dissolve them in 6mL and 15mL of 2M NaCl solution respectively, stir or ultrasonicate to make them completely dissolved, the concentration of both in NaCl solution is 0.1M; the volume ratio between the two mixed solutions is 1:2.5 to ensure that Pry-NDI is fully charged and discharged. Bubble argon for 10 minutes, and the derivatives Pry-NDI and MiAcNH-TEMPO are used as the anode electrolyte and cathode electrolyte of the battery, respectively, referred to as 0.1M Pry-NDI / 0.1MMiAcNH-TEMPO.
[0087] (2) Preparation of 0.1M diol-PryNDI / 0.1M MiAcNH-TEMPO neutral aqueous organic flow battery
[0088] Take 426mg diol-PryNDI and 495mg MiAcNH-TEMPO and dissolve them in 6mL and 15mL of 2M NaCl solution respectively, stir or ultrasonicate to make them completely dissolved, and the concentration of both in NaCl solution is 0.1M. The volume ratio between the mixed solution formed by the two is 1:2.5 to ensure that diol-PryNDI is fully charged and discharged. Bubble argon for 10 minutes, and the derivatives diol-PryNDI and MiAcNH-TEMPO are used as the battery anode electrolyte and cathode electrolyte, respectively, referred to as 0.1M diol-PryNDI / 0.1MMiAcNH-TEMPO.
[0089] Step 3: Assemble the neutral aqueous organic redox flow battery and perform performance testing;
[0090] (1) Place the fixture prepared in step 1 and the solution prepared in step 2 in a glove box, and use the prepared Pry-NDI / Prydiol-NDI solution as the negative electrode electrolyte and the MiAcNH-TEMPO solution as the positive electrode electrolyte. Connect the external power supply, peristaltic pump, and Xinwei tester, set the program, and then perform the charge and discharge test.
[0091] (2) After the above steps, the basic test data of the prepared 0.1M Pry-NDI / 0.1M MiAcNH-TEMPO system are as follows: double electron storage, voltage range 0.1~1.8V, current density 40mAcm -2 After 1000 cycles, the capacity retention rate was 97.3% and the single-cycle capacity decay rate was 0.0027%.
[0092] (3) After the above steps, the basic test data of the prepared 0.1M diol-PryNDI / 0.1M MiAcNH-TEMPO system are as follows: double electron storage, voltage range 0.1~1.8V, current density 40mAcm -2 After 1050 cycles, the capacity retention rate was 92.3% and the single-cycle capacity decay rate was 0.007%.
[0093] Therefore, the above battery tests confirm that the imide-based derivatives are an excellent negative electrode electrolyte material in neutral aqueous organic flow batteries. First, the imide molecules modified by hydrophilic groups have strong solubility in aqueous solution, which ensures that such molecules can be used in the electrolyte of neutral aqueous organic flow batteries; secondly, the imide molecules have strong conjugation, and the molecular skeleton basically does not change during the double electron transfer process, which is conducive to its double electron transfer; strong conjugation makes the band gap of naphthylimide molecules narrower, which can achieve rapid electron transfer and thus achieve stable double electron transfer. The large molecular volume avoids the intercalation of the anode electrolyte through the ion exchange membrane during the charge and discharge cycle. Compared with the more widely studied viologen molecules, the imide molecules are more conjugated and aromatic. During the double electron transfer process, the aromaticity remains basically unchanged and the molecular volume is larger. The present invention increases the water solubility of the molecule by modifying the quaternary ammonium salt and the hydroxyl group. Compared with previous studies, the water-soluble groups are increased from two to four, which further increases the water solubility of the molecule, and the increase in water-soluble groups further increases the molecular size. In the electrochemical test of double electron transfer, the neutral water-based organic redox batteries based on 0.1MPry-NDI / 0.1M MiAcNH-TEMPO and 0.1Mdiol-PryNDI / 0.1M MiAcNH-TEMPO both showed extremely strong stability. In addition, some other hydrophilic groups such as:
[0094]
[0095] (wherein the value of m is 1 to 10) etc. can also be modified to further improve the solubility and expand the molecular volume to obtain a better negative electrode electrolyte material.
[0096] The present invention conducts relevant tests on the Pry-NDI and diol-PyrNDI anode electrolyte materials prepared in the above-mentioned Examples 1 and 2. The test results are shown in the attached Figure 1 ~Attached Figure 4 .
[0097] By the attached Figure 1 The data show that the imide derivative Pry-NDI of Example 1 of the present invention has two redox peaks, which are located at -0.11V and -0.50V respectively.
[0098] By the attached Figure 2 The data show that when the imide derivative Pry-NDI of Example 1 of the present invention is used as the anode electrolyte and MiAcNH-TEMPO is used as the cathode electrolyte for double electron transfer, the voltage window of the full cell can reach 1.35V.
[0099] By the attached Figure 3The data show that in the electrochemical test of the neutral aqueous organic flow battery obtained by using 0.1M Pry-NDI, an imide derivative of Example 1 of the present invention, as the anode electrolyte and 0.1M MiAcNH-TEMPO as the cathode electrolyte, the voltage test range is 0.1V-1.8V, and when the current density is 40mA / cm 2 When the concentration is 0.1 M, the neutral aqueous organic flow battery based on Pry-NDI / MiAcNH-TEMPO shows good cycling stability over 1000 cycles; after 1000 cycles, the capacity retention rate is 97.3% and the single-cycle capacity decay rate is 0.0027%.
[0100] By the attached Figure 4 The data show that in the electrochemical test of the neutral aqueous organic flow battery obtained by using 0.1M diol-PryNDI, an imide derivative of Example 1 of the present invention, as the anode electrolyte and 0.1M MiAcNH-TEMPO as the cathode electrolyte, the voltage test range is 0.1V-1.8V, and when the current density is 40mA / cm 2 The neutral aqueous organic flow battery based on diol-PryNDI / MiAcNH-TEMPO showed good cycling stability over 1050 cycles; after 1050 cycles, the capacity retention rate was 92.3% and the single-cycle capacity decay rate was 0.007%.
[0101] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. An imide derivative, characterized in that: The imide derivative is any one of the following structural formulas: Among them, R1 is Any one of the groups; R2 is Any one of the groups; n is 1 or 2.
2. A method for preparing an imide derivative as claimed in claim 1, characterized in that: include: S1, preparation of precursor B; S2, the precursor B of step S1 reacts with Cl-R2 to obtain a reaction solution, precipitates and filters, and dries to obtain an imide derivative; The preparation of precursor B comprises: dissolving precursor A, adding Reaction to obtain precursor B; The precursor A is any one of the following structural formulas Said In the example, R1 is Any one of the groups; n is 1 or 2.
3. The method for preparing an imide derivative according to claim 2, characterized in that: The precursor A and The molar ratio is 1:
3.
4. The method for preparing an imide derivative according to claim 2, characterized in that: The solvent for dissolving the precursor A is any one of toluene, N,N-dimethylformamide and tetrahydrofuran.
5. The method for preparing an imide derivative according to claim 2, characterized in that: The molar ratio of the precursor B to Cl-R2 is 1:3; In the Cl-R2, R2 is Any one of the groups.
6. The method for preparing an imide derivative according to claim 2, characterized in that: The S2 reaction temperature is 110° C. to 130° C., and the reaction time is 22 h to 26 h.
7. The method for preparing an imide derivative according to claim 2, characterized in that: The S2 precipitate was prepared by sequentially adding ethanol and acetone according to a volume ratio of 1:10:2 of reaction solution: ethanol: acetone.
8. The method for preparing an imide derivative according to claim 2, characterized in that: The preparation of the precursor B is carried out at 110° C. to 130° C. for 20 h to 26 h.
9. The use of an imide derivative in a liquid flow battery according to claim 1, characterized in that: The liquid flow battery uses an imide derivative as an anode electrolyte and a MiAcNH-TEMPO solution as a cathode electrolyte.
10. The use of an imide derivative according to claim 9 in a neutral aqueous flow battery, characterized in that: The volume ratio of the anolyte to the cathode electrolyte is 1:2.5-3.
Citation Information
Patent Citations
STAT3-Hif1 alpha signal pathway inhibitor and application in tumor resistance thereof
CN103910727A
Imide derivative as well as preparation method and application thereof in flow battery
CN114874211A
Naphthalimide derivative, preparation method thereof and application of naphthalimide derivative in flow battery
CN116178370A
Naphthalene diimide compound and redox flow battery containing the same
US20240243327A1
Cited By
Large-scale continuous production method of diimide derivative
CN119775275A