Preparation method of nano silicon dioxide inorganic filler modified PMMA (polymethyl methacrylate) composite material
Through the combination of acyl peroxide and cationic photoinitiator, the problem of insufficient performance of inorganic nanoparticle modified PMMA composite materials is solved, and higher tensile strength, flexural strength, friction wear and hardness are achieved. This method is efficient and low-cost and is suitable for large-scale production.
Patent Information
- Application Number
- CN202411294390.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-26
AI Technical Summary
The existing inorganic nanoparticle modified PMMA composites have no obvious improvements in tensile strength, flexural strength, friction wear and hardness, and conventional initiators have resulted in incomplete reactions.
Acyl peroxide and cationic photoinitiator are used as composite initiators, polymerized under an inert gas atmosphere, and irradiated under ultraviolet light source to prepare PMMA composite materials modified with nanosilica inorganic filler.
The tensile strength, flexural strength, friction wear and hardness of PMMA composite materials are significantly improved, and the method is highly efficient, low pollution and low cost, and is suitable for large-scale production.
Smart Images

Figure BDA0005045497510000051 
Figure BDA0005045497510000052 
Figure BDA0005045497510000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biomaterials, and in particular to a method for preparing a PMMA composite material modified by a nano-silicon dioxide inorganic filler. Background Art
[0002] Polymethyl methacrylate (PMMA) is a high molecular polymer formed by free radical addition polymerization of methyl methacrylate monomers, also known as acrylic or organic glass. It has the advantages of light weight, low price, and easy molding, and is widely used. However, its application is limited by its poor surface hardness, easy scratches, poor wear resistance, and easy softening and deformation at high temperatures. In order to overcome these unfavorable factors, the prior art uses inorganic nanoparticle modification or organic polymer modification to improve the performance of polymethyl methacrylate.
[0003] Among them, when polymethyl methacrylate is modified by inorganic nanoparticles, the heat resistance, mechanical strength and impact resistance of the polymer substrate can be improved, which has become one of the directions that are widely studied. However, due to the addition of inorganic nanoparticles, there is poor compatibility between inorganic nanoparticles and polymethyl methacrylate, and when inorganic nanoparticles are used to modify polymethyl methacrylate modified with inorganic nanoparticles, when conventional initiators such as azobisisobutyronitrile are used for reaction, there is incomplete reaction, resulting in no obvious improvement in its performance in terms of tensile strength, flexural strength, friction and wear, and hardness.
[0004] In view of the problems existing in the prior art, how to provide a method for preparing an inorganic nanoparticle-modified PMMA composite material so that the prepared material has better tensile strength, flexural strength, friction and wear, and hardness is a problem to be solved urgently in the present invention. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a PMMA composite material modified by a nano-silicon dioxide inorganic filler, so as to solve the problem that the tensile strength, flexural strength, friction and wear and hardness of the inorganic nanoparticle-modified PMMA composite material prepared in the prior art are poor.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a PMMA composite material modified by a nano-silicon dioxide inorganic filler, comprising the following steps:
[0008] (1) placing the modified nano-silica and methyl methacrylate monomer in a reactor and stirring to uniformly mix;
[0009] (2) adding a composite initiator to step (1) and polymerizing under an inert gas atmosphere to obtain a composite resin intermediate;
[0010] (3) placing the composite resin intermediate obtained in step (2) under an ultraviolet light source for irradiation reaction to obtain a PMMA composite material modified with a nano-silicon dioxide inorganic filler;
[0011] The composite initiator comprises initiator 1 and initiator 2;
[0012] The first initiator is an acyl peroxide initiator, and the second initiator is a cationic photoinitiator.
[0013] Initiator 1 is an acyl peroxide initiator, and initiator 2 is a cationic photoinitiator. When they are used together to prepare a PMMA composite material modified with nano-silica inorganic filler, it has the characteristics of high reaction efficiency, energy saving, and environmental friendliness, and improves the flexural strength, wear resistance and hardness of PMMA.
[0014] As a further improvement, the wavelength band of the ultraviolet light source in step (3) is 280-400nm.
[0015] As a further improvement, the weight ratio of initiator 1 to initiator 2 is 2-5:1.
[0016] As a further improvement, the added amount of the composite initiator is 1-3 wt % of the methyl methacrylate monomer.
[0017] In order to have better wear resistance and better tensile strength, preferably, the cationic photoinitiator is prepared by reacting 2-mercaptobenzoxazole, 1,4-diiodobenzene and diphenyliodonium trifluoromethanesulfonate.
[0018] As a further improvement, the method for preparing the cationic photoinitiator comprises the following steps:
[0019] In a flask, 2-mercaptobenzoxazole and 1,4-diiodobenzene are added in sequence and dissolved with an organic solvent, and then cuprous iodide and an inorganic base are added. The flask is placed in a microwave reactor for sufficient reaction. After the reaction is completed, post-treatment is performed to obtain an intermediate 1. Subsequently, the intermediate 1 and diphenyliodonium trifluoromethanesulfonate are dissolved with an organic solvent, and then cuprous iodide and metal powder are added to react. The reaction temperature is 100-120°C. After the reaction is completed, post-treatment is performed to obtain a cationic photoinitiator.
[0020] As a further improvement, the molar ratio of 2-mercaptobenzoxazole to 1,4-diiodobenzene is 1.5-3:1;
[0021] The molar ratio of the intermediate 1 to diphenyliodonium trifluoromethanesulfonate is 1:2-4.
[0022] As a further improvement, the initiator 1 is at least one of benzoyl peroxide and lauroyl peroxide.
[0023] As a further improvement, the weight ratio of the modified nano-silica to the methyl methacrylate monomer is 1-10:90-99.
[0024] As a further improvement, the modified nano-silica in step (1) is nano-silica modified by a silane coupling agent.
[0025] As a further improvement, the silane coupling agent is at least one of KH-550, KH-570, WD-56, and WD-71.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The PMMA composite material modified with nano-silicon dioxide inorganic filler prepared by the preparation method provided by the present invention has better tensile strength, flexural strength, friction and wear, and hardness. The preparation method of the present invention is efficient, low-pollution, low-cost, has low requirements on equipment, and is suitable for large-scale production. DETAILED DESCRIPTION
[0028] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0029] In the following examples, except for modified nano-silica A and cationic photoinitiator A, the other compound monomers and related reagents used can be purchased from the market, among which nano-silica (particle size of 20 nm) was purchased from Nanjing Tianxing New Materials Co., Ltd., model TSP-H10.
[0030] The preparation method of modified nano silicon dioxide A comprises the following steps:
[0031] Accurately weigh 5 g of nano-silica powder and add it to a 500 mL round-bottom flask, then add 200 mL of anhydrous ethanol, ultrasonically disperse for 30 min, drop 1.0 g of KH-570 coupling agent, and then heat to 80 ° C., reflux for 2 h, centrifuge, wash, and vacuum dry to obtain modified nano-silica A.
[0032] The preparation steps of cationic photoinitiator A are as follows:
[0033] In a 100 mL long-necked flask, 2.2 mmol 2-mercaptobenzoxazole and 1 mmol 1,4-diiodobenzene were added in sequence, dissolved with 4 mL N,N-dimethylamide, and then 0.1 mmol cuprous iodide and 15 mmol potassium hydroxide were added. The flask was placed in a microwave reactor, the power was set to 30 W, and the reaction was carried out for 20 min. After the flask was cooled to room temperature, the reaction mixture was transferred to a separatory funnel, extracted with ethyl acetate, and the solvent in the organic phase was dried to obtain a crude product. The crude product was separated by column chromatography with V (petroleum ether): V (ethyl acetate) = 1:20 to obtain intermediate 1;
[0034] Next, 1 mmol of intermediate 1 and 2.4 mmol of diphenyliodonium trifluoromethanesulfonate were added in sequence to a 50 mL round-bottom flask equipped with a stirrer, dissolved with 2 mL of 1,1,2,2-tetrachloroethane, and then 0.1 mmol of cuprous iodide and 0.1 mmol of copper powder were added. The temperature was raised to 110°C and the reaction was carried out for 2 h. After the reaction liquid was cooled to room temperature, the solvent was removed and column chromatography was performed to obtain cationic photoinitiator A.
[0035] The preparation methods of Examples 1-5 and Comparative Examples 2-3 comprise the following steps:
[0036] (1) Stirring the modified nano-silica A and methyl methacrylate monomer until they are uniformly mixed at a stirring speed of 500 rpm;
[0037] (2) adding a composite initiator to step (1), and polymerizing under a nitrogen atmosphere at a stirring speed of 700 rpm, a temperature of 85-90° C., and a stirring time of 30 min to obtain a composite resin intermediate;
[0038] (3) placing the composite resin intermediate obtained in step (2) under an ultraviolet light source for irradiation reaction to obtain a PMMA composite material modified with nano-silicon dioxide inorganic filler, wherein the light source has a wavelength of 280-295 nm and the irradiation reaction lasts for 20 minutes.
[0039] The preparation method of Comparative Example 1 comprises the following steps:
[0040] (1) stirring nano-silica and methyl methacrylate monomer until they are uniformly mixed, and the stirring speed during mixing is 500 rpm;
[0041] (2) adding a composite initiator to step (1), and polymerizing under a nitrogen atmosphere at a stirring speed of 700 rpm, a temperature of 85-90° C., and a stirring time of 30 min to obtain a composite resin intermediate;
[0042] (3) placing the composite resin intermediate obtained in step (2) under an ultraviolet light source for irradiation reaction to obtain a PMMA composite material modified with nano-silicon dioxide inorganic filler, wherein the light source has a wavelength of 280-295 nm and the irradiation reaction lasts for 20 minutes.
[0043] The components and contents used in Examples 1-5 and Comparative Examples 1-3 are shown in Table 1-2 below:
[0044] Table 1
[0045]
[0046] Table 2
[0047]
[0048]
[0049] The tensile strength, flexural strength, friction and wear, and hardness of the PMMA composite materials modified with nano-silicon dioxide inorganic fillers obtained in Examples 1-5 and Comparative Examples 1-3 were tested as follows:
[0050] 1. Tensile strength: According to GB / T1040.2-2006, the test speed is 5mm / min, and the specimen is 1A dumbbell specimen;
[0051] 2. Flexural performance test: According to GB / T9341-2008, the test speed is 2mm / min, and the sample size is 80mm×10mm×4mm;
[0052] 3. Friction and wear test: According to GB / T 3960-2016, the test ring rotates at 200rpm, the test is repeated 3 times and the average value is taken. The sample size is 30mm×7mm×6mm;
[0053] 4.Hardness test: According to GB / T3398.2-2008, the sample size is 10mm×10mm×4mm.
[0054] The measured results are shown in Table 3:
[0055] Table 3
[0056]
[0057]
[0058] It can be seen from Examples 1-5 and Comparative Example 1 in Table 3 that the tensile strength, flexural strength, friction and wear, and hardness of the PMMA composite material prepared from modified nano-silica are superior to those of the PMMA composite material prepared from unmodified nano-silica.
[0059] It can be seen from the test results of Example 2 and Comparative Examples 2-3 that the mechanical properties of the PMMA composite materials modified with nano-silica inorganic fillers prepared by using an acyl peroxide initiator and a cationic photoinitiator are better than the mechanical properties of the PMMA composite materials modified with nano-silica inorganic fillers prepared by using a conventional initiator and a cationic photoinitiator or a conventional initiator and an acyl peroxide initiator.
[0060] It can be seen from the test results of Examples 1-3 and Examples 4-5 that when the weight ratio of initiator 1 to initiator 2 is within an appropriate range, the tensile strength, flexural strength, friction and wear, and hardness of the PMMA composite material modified with nano-silica inorganic filler are all excellent.
[0061] It can be seen from the test results of Examples 1-3 that the PMMA composite material modified with nano-silicon dioxide inorganic filler prepared by the preparation method provided by the present invention has better tensile strength, flexural strength, friction and wear, and hardness.
[0062] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a PMMA composite material modified with nano-silicon dioxide inorganic filler, It is characterized in that The following steps are involved: (1) placing modified nano-silica and methyl methacrylate monomer in a reactor and stirring until uniformly mixed; (2) adding a composite initiator to step (1) and polymerizing under an inert gas atmosphere to obtain a composite resin intermediate; (3) placing the composite resin intermediate obtained in step (2) under an ultraviolet light source for irradiation reaction to obtain a PMMA composite material modified with a nano-silicon dioxide inorganic filler; The composite initiator comprises initiator 1 and initiator 2; The first initiator is an acyl peroxide initiator, and the second initiator is a cationic photoinitiator.
2. A method for preparing a PMMA composite material modified with nano-silicon dioxide inorganic filler according to claim 1, It is characterized in that The weight ratio of the initiator 1 to the initiator 2 is 2-5:
1.
3. A method for preparing a PMMA composite material modified with nano-silicon dioxide inorganic filler according to claim 1, It is characterized in that The added amount of the composite initiator is 1-3 wt % of the methyl methacrylate monomer.
4. A method for preparing a PMMA composite material modified with nano-silicon dioxide inorganic filler according to claim 1 or 2, It is characterized in that The cationic photoinitiator is prepared by reacting 2-mercaptobenzoxazole, 1,4-diiodobenzene and diphenyliodonium trifluoromethanesulfonate.
5. A method for preparing a PMMA composite material modified with nano-silicon dioxide inorganic filler according to claim 1, It is characterized in that The preparation method of the cationic photoinitiator comprises the following steps: In a flask, 2-mercaptobenzoxazole and 1,4-diiodobenzene are added in sequence and dissolved with an organic solvent, and then cuprous iodide and an inorganic base are added. The flask is placed in a microwave reactor for sufficient reaction. After the reaction is completed, post-treatment is performed to obtain an intermediate 1. Subsequently, the intermediate 1 and diphenyliodonium trifluoromethanesulfonate are dissolved with an organic solvent, and then cuprous iodide and metal powder are added to react. The reaction temperature is 100-120°C. After the reaction is completed, post-treatment is performed to obtain a cationic photoinitiator.
6. A method for preparing a PMMA composite material modified with nano-silicon dioxide inorganic filler according to claim 5, It is characterized in that The molar ratio of 2-mercaptobenzoxazole to 1,4-diiodobenzene is 1.5-3:1; The molar ratio of the intermediate 1 to diphenyliodonium trifluoromethanesulfonate is 1:2-4.
7. A method for preparing a PMMA composite material modified with nano-silicon dioxide inorganic filler according to claim 1, It is characterized in that The first initiator is at least one of benzoyl peroxide and lauroyl peroxide.
8. A method for preparing a PMMA composite material modified with nano-silicon dioxide inorganic filler according to claim 1, It is characterized in that The weight ratio of the modified nano-silica to the methyl methacrylate monomer is 1-10:90-99.
9. The method for preparing a PMMA composite material modified by a nano-silicon dioxide inorganic filler according to claim 1, It is characterized in that The modified nano-silica in the step (1) is nano-silica modified by a silane coupling agent.