Artificial SEI material, lithium metal battery negative electrode, battery and preparation method and application of artificial SEI material

The lithium metal battery cycle was solved by applying artificial SEI materials prepared from 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and terephthalaldehyde to the negative electrode surface of the lithium metal battery. The problems of poor stability and low Coulomb efficiency achieve a more uniform lithium deposition and peeling process, significantly improving the electrochemical performance of the battery.

CN119019628AInactive Publication Date: 2024-11-26SHANGHAI JIAOTONG UNIV

Patent Information

Application Number
CN202411140839.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The poor cycle stability of lithium metal batteries and low Coulomb efficiency are mainly due to the high reactivity of lithium metal, which leads to irreversible reactions in the electrolyte, resulting in a thicker SEI layer, which consumes lithium and electrolyte, causing rapid attenuation of cycle stability performance. and low Coulomb efficiency.

Method used

Artificial SEI material prepared by reacting 2,4,6-tri(4-aminophenyl)-1,3,5-triazine and fluorine substitute of terephthalaldehyde through Schiff base, coated on lithium metal battery On the surface of the negative electrode, a stable SEI layer is formed, reducing the side reactions of lithium metal interfaces and improving cyclic stability and electrochemical properties.

Benefits of technology

By forming excellent electrochemical stability, local current density is reduced, critical current density is improved, uniform deposition of lithium, inhibit the formation of lithium dendrites, and significantly improve the cyclic stability and Coulomb efficiency of lithium metal batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019628A_ABST
    Figure CN119019628A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium batteries, and discloses an artificial SEI material, a lithium metal battery negative electrode, a battery and a preparation method and application thereof. The preparation method of the artificial SEI material comprises the following steps: dissolving a monomer A and a monomer B in a solvent A, and adding a catalyst to obtain a mixed solution; wherein the monomer A is 2, 4, 6-tri (4-aminophenyl)-1, 3, 5-triazine, and the monomer B is a fluorine substitute of terephthalaldehyde; sequentially freezing, degassing and unfreezing the mixed solution, then heating under vacuum to react, collecting a solid phase, washing, purifying and drying to obtain the artificial SEI material. The artificial SEI material is used for the negative electrode of the lithium metal battery, so that the side reaction of a lithium metal interface can be effectively reduced, a stable lithium metal deposition / stripping process is realized, and the cycling stability of the lithium metal battery is improved. The artificial SEI material has excellent electrochemical stability, and can reduce local current density, improve critical current density, promote uniform deposition of lithium and inhibit formation of lithium dendrites.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium batteries, and in particular to an artificial SEI material, a lithium metal battery negative electrode, a battery, and a preparation method and application thereof. Background Art

[0002] Traditional lithium-ion batteries have reached their energy density limit (≈300Wh kg -1 ), which is difficult to meet the growing demand for battery performance. The theoretical specific capacity of graphite, the negative electrode material of lithium-ion batteries, is only 372mAh g -1 , which greatly restricts the improvement of lithium-ion battery energy density. Lithium metal anode has a high theoretical specific capacity (3860mAh g -1 ), which is about 10 times that of graphite, and lithium metal has an extremely low reduction potential (-3.04V vs SHE), which is considered to be an ideal negative electrode material. Therefore, lithium metal batteries with lithium metal as negative electrode material have attracted much attention due to their high energy density.

[0003] However, lithium metal anode still has a series of shortcomings and deficiencies, resulting in poor battery cycle performance and low coulombic efficiency, which limits its application. Its failure is mainly caused by the following reasons: lithium metal has high reactivity and is prone to irreversible continuous reaction with electrolyte, forming a thick SEI layer on the surface of lithium metal, consuming lithium and electrolyte, resulting in rapid decay of cycle stability performance and low coulombic efficiency.

[0004] Building a stable SEI layer on the surface of lithium metal anode is considered to be one of the effective strategies to improve the interfacial performance of lithium metal. Based on this, this application develops an artificial SEI material to enhance the cycle stability of lithium metal batteries. Summary of the invention

[0005] The present application provides an artificial SEI material, a lithium metal battery negative electrode, a battery and a preparation method and application thereof, aiming to solve the problems of poor cycle stability and low coulombic efficiency in existing lithium metal batteries.

[0006] In order to achieve the above objectives, the present application adopts the following technical solutions.

[0007] In a first aspect of the present application, a method for preparing an artificial SEI material is provided, comprising:

[0008] S1, dissolving monomer A and monomer B in solvent A, and then adding a catalyst to obtain a mixed solution;

[0009] Wherein, the monomer A is 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, and the monomer B is a fluorine-substituted product of terephthalaldehyde;

[0010] S2, freezing, degassing and thawing the mixed solution in sequence, then heating under vacuum for reaction, collecting the solid phase, washing, purifying and drying to obtain the artificial SEI material.

[0011] In some embodiments, the monomer B includes any one of 2,3-difluoroterephthalaldehyde, 2,5-difluoroterephthalaldehyde, or 2,3,5,6-tetrafluoroterephthalaldehyde.

[0012] In some embodiments, the molar ratio of monomer A to monomer B is 1:(1-3).

[0013] In some embodiments, the solvent A is a mixed solvent of mesitylene and dioxane in a volume ratio of 1:(1-10);

[0014] The catalyst is glacial acetic acid;

[0015] The molar ratio of the catalyst to the monomer A is (100-1000):1.

[0016] In some embodiments, the freezing temperature is -100°C to -50°C; the degassing is performed by vacuuming;

[0017] and / or:

[0018] The reaction temperature is 100-160° C., the reaction vacuum is 200-300 Pa, and the reaction time is 48-96 hours.

[0019] The second aspect of the present application provides an artificial SEI material prepared by the above preparation method.

[0020] In a third aspect of the present application, a negative electrode for a lithium metal battery is provided, comprising lithium metal and a SEI layer coated on a surface of the lithium metal;

[0021] The SEI layer includes the artificial SEI material, a binder and a solvent B.

[0022] In a fourth aspect of the present application, a method for preparing a negative electrode of a lithium metal battery is provided, characterized in that it comprises:

[0023] The artificial SEI material, the binder and the solvent are uniformly mixed in a mass ratio of 10:(1-4):(100-300) to obtain a slurry;

[0024] The slurry is coated on the surface of lithium metal and vacuum dried to obtain the negative electrode of lithium metal battery.

[0025] In some embodiments, the binder includes any one of polybutylene rubber, styrene butadiene rubber, carboxymethyl cellulose or polyvinylidene fluoride;

[0026] The solvent B includes any one of n-hexane, xylene, mesitylene or benzyl acetate.

[0027] In a fifth aspect of the present application, a lithium metal battery is provided, wherein the negative electrode thereof is the negative electrode of the lithium metal battery described above.

[0028] Compared with the prior art, the beneficial effects of this application are:

[0029] The artificial SEI material prepared by the Schiff base reaction of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and the fluorine-substituted product of terephthalaldehyde has excellent electrochemical stability, can reduce the local current density, increase the critical current density, promote the uniform deposition of lithium and inhibit the formation of lithium dendrites.

[0030] The artificial SEI material of the present application is used for the negative electrode of lithium metal battery, which can effectively reduce the side reaction of lithium metal interface, realize the stable lithium metal deposition / stripping process, and improve the cycle stability of lithium metal battery. + It has strong attraction ability, increases the lithium-philic sites of the framework material, can significantly improve the ionic conductivity and lithium ion migration number of the material, and provide Li + Fast transmission channel, thus uniform Li + The deposition and stripping process can reduce the occurrence of lithium metal interface side reactions and the formation of lithium dendrites, thereby improving the electrochemical performance of lithium metal batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments recorded in the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0032] Figure 1 This is the XRD test spectrum of the artificial SEI material prepared in Example 1;

[0033] Figure 2 This is a graph showing the long cycle charge and discharge test results of the lithium metal batteries assembled in Example 6 and Comparative Example 1. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0035] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.

[0036] In the following description of this embodiment, the term "and / or" is used to describe the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, B exists alone, and A and B exist at the same time. A and B can be singular or plural. The character " / " generally indicates that the associated objects before and after are in an "or" relationship.

[0037] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0038] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0039] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0040] Those skilled in the art will appreciate that the numerical ranges in the embodiments of the present application are to be construed as specifically disclosing each intermediate value between the upper and lower limits of the scope. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present application. The upper and lower limits of these smaller ranges may be independently included or excluded in the scope.

[0041] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which this application belongs. Although this application only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of this application. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0042] In a first aspect, the present application provides a method for preparing an artificial SEI material, comprising:

[0043] S1, dissolving monomer A and monomer B in a solvent, and then adding a catalyst to obtain a mixed solution;

[0044] Wherein, the monomer A is 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, and the monomer B is a fluorine-substituted product of terephthalaldehyde, and preferably the number of fluorine substituents in the monomer B is two or more.

[0045] Specifically, the monomer B can be any one of 2,3-difluoroterephthalaldehyde, 2,5-difluoroterephthalaldehyde or 2,3,5,6-tetrafluoroterephthalaldehyde.

[0046] The solvent is a mixed solvent of non-polar mesitylene and polar dioxane, which is conducive to the dispersion of monomer A and monomer B. By adjusting the polarity range of the reaction, the dispersion of the monomers is improved, and the crystallinity of the product can be improved. The preferred volume ratio of mesitylene to dioxane in the present application is 1: (1-10), and the more preferred volume ratio is 1: (1-5).

[0047] The catalyst is glacial acetic acid, preferably a glacial acetic acid aqueous solution with a molar concentration of 2-12M; the catalyst can catalyze the Schiff base reaction of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and the fluorine-substituted product of terephthalaldehyde, and make the generated CTF material connected by imine bond have better crystallinity.

[0048] In the examples of the present application, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and fluorine-substituted terephthalaldehyde are added to a heat-resistant glass container, and mesitylene, dioxane and glacial acetic acid are added, and ultrasonic treatment is performed to obtain a mixed solution.

[0049] S2, freezing, degassing and thawing the mixed solution in sequence, then heating under vacuum for reaction, collecting the solid phase, washing, purifying and drying to obtain the artificial SEI material.

[0050] The present invention freezes the mixed solution at -100°C to -50°C, then degasses it by vacuuming it three times, and then thaws it. The above steps remove the residual gas in the mixed solution, further improve the crystallinity of the reaction product, and adjust the pore distribution in the reaction product.

[0051] The mixed solution after freezing, degassing and thawing is sealed and evacuated to 200-300 Pa, heated to 100-160°C, and reacted for 48-96 hours. After the reaction, the solid phase is collected as a crude product. The crude product is washed with alcohol and ketone solvents, wherein the alcohol solvent includes methanol, ethanol or a mixture thereof; the ketone solvent is preferably acetone. The washed crude product is purified by a Soxhlet extractor with acetone as a solvent to remove oligomers, and the CTF material, i.e., artificial SEI material, is obtained after drying. In the present application, the molar ratio of monomer A to monomer B is preferably 1:(1-3), and the molar ratio of catalyst to monomer A is (100-1000):1. Taking monomer A as 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and monomer B as 2,3-difluoroterephthalaldehyde as an example, the reaction formula for synthesizing CTF is:

[0052]

[0053] The applicant has found that using the CTF material prepared in this application as an artificial SEI layer for the negative electrode of a lithium metal battery can effectively reduce the side reactions at the lithium metal interface, achieve a stable lithium metal deposition / stripping process, and improve the cycle stability of the lithium metal battery. The reason is that: on the one hand, F and C=N bonds are not conducive to Li + It has strong attraction ability, increases the lithium-philic sites of the framework material, can significantly improve the ionic conductivity and lithium ion migration number of the material, and provide Li + Fast transmission channel, thus uniform Li + The deposition and stripping process of lithium metal can reduce the occurrence of side reactions at the lithium metal interface and the formation of lithium dendrites, thereby improving the electrochemical performance of lithium metal batteries. On the other hand, CTF materials have excellent electrochemical stability, can reduce local current density, increase critical current density, further promote uniform deposition of lithium and inhibit the formation of lithium dendrites. The artificial SEI layer of this application realizes a stable lithium metal deposition / stripping process.

[0054] The present application also provides a lithium metal battery negative electrode, which comprises lithium metal and a SEI layer coated on the surface of the lithium metal; the SEI layer comprises the above-mentioned artificial SEI material, a binder and a solvent.

[0055] Wherein, the lithium metal can be pure lithium or lithium alloy, and its shape can be sheet or strip, and there is no special restriction on it. The solvent is used to disperse the artificial SEI material, and any one of n-hexane, xylene, mesitylene or benzyl acetate can be selected. The binder is used to improve the bonding strength between the artificial SEI material and the lithium metal, and any one of polybutylene rubber, styrene butadiene rubber, carboxymethyl cellulose and polyvinylidene fluoride can be selected.

[0056] The method for preparing the negative electrode of a lithium metal battery of the present application comprises:

[0057] The artificial SEI material, the binder and the solvent are mixed evenly in a mass ratio of 10:(1-4):(100-300) to obtain a slurry; the slurry is then applied to the surface of the lithium metal, and vacuum dried to obtain a negative electrode of a lithium metal battery. In the present application, the coating method is preferably scraping.

[0058] The present application also provides a lithium metal battery, whose negative electrode is the negative electrode of the lithium metal battery described above. In addition to the lithium metal battery negative electrode described in the present application, the other component materials and structures of the lithium metal battery described in the present application can be conventional. For example, the positive electrode active material of the lithium metal battery includes at least one of lithium nickel cobalt manganese oxide, lithium manganese phosphate, lithium titanate, lithium iron phosphate, lithium nickel oxide, lithium manganese oxide, and lithium cobalt oxide; the electrolyte can be selected from at least one of an ether-based electrolyte of a lithium salt or a carbonate electrolyte, wherein the lithium salt includes at least one of lithium nitrate, lithium perchlorate, lithium hexafluorophosphate, and lithium bis(trifluoromethanesulfonyl)imide.

[0059] The present application is further described below by way of examples.

[0060] Example 1

[0061] This embodiment provides a method for preparing an artificial SEI material, wherein the monomer A is 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, and the monomer B is 2,3-difluoroterephthalaldehyde. Specifically, the method includes:

[0062] 1.2 mmol of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and 1.8 mmol of 2,3-difluoroterephthalaldehyde were added to a heat-resistant glass container, and then 12 mL of mesitylene, 12 mL of dioxane and 40 mL of glacial acetic acid solution with a molar concentration of 12 M were added, and stirred evenly to obtain a mixed solution;

[0063] The mixed solution was cooled to -70°C for freezing and vacuumed for 3 times; after thawing, the solution was vacuumed to a pressure of 200 Pa and heated to 120°C for reaction for 72 hours. After the reaction, the solid phase was collected by centrifugation, and the solid phase powder was washed with methanol and acetone for 3 times each, purified by Soxhlet extractor, and dried at 60°C to obtain an artificial SEI material.

[0064] Example 2

[0065] This embodiment provides a method for preparing an artificial SEI material, wherein the monomer A is 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, and the monomer B is 2,3-difluoroterephthalaldehyde. Specifically, the method includes:

[0066] 1.2 mmol of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and 2.4 mmol of 2,3-difluoroterephthalaldehyde were added to a heat-resistant glass container, and then 12 mL of mesitylene, 12 mL of dioxane and 10 mL of glacial acetic acid solution with a molar concentration of 12 M were added, and stirred evenly to obtain a mixed solution;

[0067] The mixed solution was cooled to -50°C for freezing and vacuumed for 3 times; after thawing, the solution was vacuumed to a pressure of 300 Pa and heated to 120°C for reaction for 72 hours. After the reaction, the solid phase was collected by centrifugation, and the solid phase powder was washed with methanol and acetone for 3 times each, purified by Soxhlet extractor, and dried at 60°C to obtain an artificial SEI material.

[0068] Example 3

[0069] This embodiment provides a method for preparing an artificial SEI material, wherein the monomer A is 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, and the monomer B is 2,3-difluoroterephthalaldehyde. Specifically, the method includes:

[0070] 1.2 mmol of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and 3.6 mmol of 2,3-difluoroterephthalaldehyde were added to a heat-resistant glass container, and then 12 mL of mesitylene, 60 mL of dioxane and 100 mL of glacial acetic acid solution with a molar concentration of 12 M were added, and stirred evenly to obtain a mixed solution;

[0071] The mixed solution was cooled to -100°C for freezing and vacuumed for 3 times; after thawing, the solution was vacuumed to a pressure of 200 Pa and heated to 120°C for reaction for 72 hours. After the reaction, the solid phase was collected by centrifugation, and the solid phase powder was washed with methanol and acetone for 3 times each, purified by Soxhlet extractor, and dried at 80°C to obtain an artificial SEI material.

[0072] Example 4

[0073] The difference between Example 4 and Example 1 is that monomer B is replaced by 2,5-difluoroterephthalaldehyde, and the rest is the same as Example 1.

[0074] Example 5

[0075] The difference between Example 5 and Example 1 is that monomer B is replaced by 2,3,5,6-tetrafluoroterephthalaldehyde, and the rest is the same as Example 1.

[0076] The artificial SEI material prepared in Example 1 was subjected to XRD test, and its test spectrum is as follows: Figure 1 As shown. Figure 1 It can be seen that the artificial SEI material prepared in Example 1 has good crystallinity.

[0077] The XRD test results of the artificial SEI materials of Examples 2 to 5 show that they all have good crystallinity.

[0078] Example 6

[0079] This embodiment provides a CR2032 button battery with an SEI layer on the negative electrode surface, wherein the negative electrode is a lithium sheet with an SEI layer. The preparation method thereof comprises:

[0080] LiFePO4, polyvinylidene fluoride and acetylene black were mixed in NMP at a mass ratio of 8:1:1 to form a slurry, the slurry was coated on Al foil, vacuum dried at 80°C, and then punched into 12 mm discs to obtain a positive electrode sheet;

[0081] The artificial SEI material, polyvinylidene fluoride and 1,4-dioxane were mixed in a mass ratio of 9:1:100 to obtain a slurry, which was scraped onto a lithium sheet, dried in a vacuum oven at 80°C, and then punched into a 14 mm disc to obtain a negative electrode sheet (CTF@Li);

[0082] Dissolving lithium bis(trifluoromethanesulfonyl imide) in a mixed solution of dimethyl ether and 1,3-dioxolane (volume ratio of 1:1) to prepare a lithium bis(trifluoromethanesulfonyl imide solution with a molar concentration of 1 M as an electrolyte;

[0083] A CR2032 button cell was assembled using the positive electrode sheet, negative electrode sheet, electrolyte and polypropylene separator, and was recorded as lithium metal battery 1.

[0084] Comparative Example 1

[0085] Comparative Example 1 provides a CR2032 button battery without a SEI layer on the negative electrode surface, wherein the negative electrode is a lithium sheet.

[0086] The preparation method thereof comprises:

[0087] LiFePO4, polyvinylidene fluoride and acetylene black were mixed in NMP at a mass ratio of 8:1:1 to form a slurry, the slurry was coated on Al foil, vacuum dried at 80°C, and then punched into 12 mm discs to obtain a positive electrode sheet;

[0088] Dissolving lithium bis(trifluoromethanesulfonyl imide) in a mixed solution of dimethyl ether and 1,3-dioxolane (volume ratio of 1:1) to prepare a lithium bis(trifluoromethanesulfonyl imide solution with a molar concentration of 1 M as an electrolyte;

[0089] A CR2032 button cell was assembled using the above-mentioned positive electrode sheet, lithium sheet, electrolyte and polypropylene separator, and was recorded as lithium metal battery D1.

[0090] The lithium metal battery 1 and lithium metal battery D1 assembled from Example 6 and Comparative Example 1 were subjected to a long cycle charge and discharge test, with the rate set to 0.5C. The results are shown in FIG. Figure 2 shown.

[0091] Depend on Figure 2 It can be seen that the initial charge capacity of the lithium metal battery 1 (CTF@Li) with SEI layer reaches 165.7 mAh g -1 The initial discharge capacity reaches 151.1 mAh g -1 , the initial coulombic efficiency is 91.2%, and after 200 cycles, the capacity retention rate is 77.6%. The initial coulombic efficiency of the lithium metal battery D1 without SEI layer under the same conditions is only 88.7%, and after 200 cycles, the capacity decays to 55.1%. After the SEI layer prepared by the artificial SEI material of the present application is added to the negative electrode of the lithium metal battery, the initial coulombic efficiency is significantly improved, and the cycle stability is greatly improved. The artificial SEI material of the present application is used as an artificial SEI layer for lithium protection, which can effectively reduce the side reactions between lithium metal and electrolyte, achieve more uniform lithium deposition, and inhibit the formation of lithium dendrites, thereby greatly improving the initial coulombic efficiency of the lithium metal battery and improving the stability of the battery during the cycle.

[0092] Although the present application has been described in detail in general terms and in specific embodiments in this specification, it is obvious to those skilled in the art that some modifications or improvements may be made to the present application. Therefore, these modifications or improvements made without departing from the spirit of the present application are within the scope of protection claimed in the present application.

Claims

1. A method for preparing an artificial SEI material, It is characterized in that include: S1, dissolving monomer A and monomer B in solvent A, and then adding a catalyst to obtain a mixed solution; Wherein, the monomer A is 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, and the monomer B is a fluorine-substituted product of terephthalaldehyde; S2, freezing, degassing and thawing the mixed solution in sequence, then heating under vacuum for reaction, collecting the solid phase, washing, purifying and drying to obtain the artificial SEI material.

2. The method for preparing the artificial SEI material according to claim 1, It is characterized in that The monomer B includes any one of 2,3-difluoroterephthalaldehyde, 2,5-difluoroterephthalaldehyde or 2,3,5,6-tetrafluoroterephthalaldehyde.

3. The method for preparing the artificial SEI material according to claim 1, It is characterized in that The molar ratio of monomer A to monomer B is 1:(1-3).

4. The method for preparing the artificial SEI material according to claim 1, It is characterized in that The solvent A is a mixed solvent of mesitylene and dioxane in a volume ratio of 1:(1-10); The catalyst is glacial acetic acid; The molar ratio of the catalyst to the monomer A is (100-1000):

1.

5. The method for preparing the artificial SEI material according to claim 1, It is characterized in that The freezing temperature is -100°C to -50°C; the degassing is performed by vacuuming; and / or: The reaction temperature is 100-160° C., the reaction vacuum is 200-300 Pa, and the reaction time is 48-96 hours.

6. An artificial SEI material prepared by the preparation method according to any one of claims 1 to 5.

7. A lithium metal battery negative electrode, It is characterized in that It includes lithium metal and a SEI layer coated on the surface of the lithium metal; The SEI layer comprises the artificial SEI material according to claim 6, a binder and a solvent B.

8. The method for preparing a negative electrode for a lithium metal battery according to claim 7, It is characterized in that include: The artificial SEI material according to claim 6, the binder and the solvent are uniformly mixed in a mass ratio of 10:(1-4):(100-300) to obtain a slurry; The slurry is coated on the surface of lithium metal and vacuum dried to obtain the negative electrode of lithium metal battery.

9. The method for preparing a negative electrode for a lithium metal battery according to claim 8, It is characterized in that The binder includes any one of polybutene rubber, styrene butadiene rubber, carboxymethyl cellulose or polyvinylidene fluoride; The solvent B includes any one of n-hexane, xylene, mesitylene or benzyl acetate.

10. A lithium metal battery, It is characterized in that The negative electrode is the negative electrode of the lithium metal battery as claimed in claim 7.

Citation Information

Patent Citations

  • Lithium battery electrode and preparation method and application thereof

    CN114388731A

  • Silicon-based composite negative electrode material and preparation method thereof

    CN115101730A

  • Preparation method and application of lithium negative electrode based on covalent organic framework material modification

    CN115403723A

  • Composition for electrode, electrode for battery, lithium secondary battery, and method of manufacturing lithium secondary battery

    JP2010009917A

  • Covalent organic frameworks and applications thereof in chemical reactions

    US20230001397A1

Cited By

  • Preparation method of covalent triazine framework material constructed by metal disulfide alkene complex and all-solid-state battery application of covalent triazine framework material