Modified titanium catalyst as well as preparation method and application thereof
By designing a modified titanium catalyst, cobalt acetate and second metal acetate react with organic titanate to form a catalyst with a bititanium ring structure, which solves the problem of catalyzing terephthalate polyester when titanium-based catalysts are catalyzed The thermal degradation and hue change problems improve the viscosity and hue stability of polyester.
Patent Information
- Application Number
- CN202411044104.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-26
AI Technical Summary
When the existing titanium catalysts catalyze the thermal degradation reaction when catalyzing the polycondensation reaction of terephthalate polyester, it will cause difficulty in increasing the viscosity and produce side reactions during the catalysis process, resulting in a difference in hue phase change.
Using a modified titanium catalyst, its structure includes 1 to 7 alkylene groups and coordination metals cobalt, zinc, manganese, and magnesium. The catalyst is formed by reacting cobalt acetate and the second metal acetate with organic titanate. The precursor suspension was centrifuged, washed and dried to produce a modified titanium catalyst for esterification and polycondensation reaction of terephthalate polyester.
The catalytic efficiency is improved, the viscosity and hue stability of the polyester are enhanced, thermal degradation and side reactions are avoided, and efficient catalytic and hue optimization are achieved.
Smart Images

Figure BDA0004973049820000021 
Figure BDA0004973049820000101 
Figure FDA0004973049810000011
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of poly(terephthalate)-based polyester preparation, and in particular to a modified titanium catalyst and a preparation method and application thereof. Background Art
[0002] Polyester is a general term for polymers obtained by polycondensation of dibasic acids and diols. Since its introduction, it has attracted widespread attention due to its advantages such as high strength, corrosion resistance, and strong plasticity. Today, polyester materials are not only widely used in traditional fields such as textile fibers, films, bottled containers, automobiles, and electronics, but also have outstanding performance in many emerging fields such as national defense science and technology, aerospace, and communications. There are many types of polyester materials, among which polyesters with terephthalic acid as raw material and building block account for an absolute proportion. This is not only because terephthalic acid raw materials are easy to obtain and low in cost, but also related to the excellent performance of its downstream materials.
[0003] The industrial production of terephthalic acid-based polyester is mainly based on the direct esterification-polycondensation process of terephthalic acid and diols, in which both the esterification and polycondensation processes require the participation of catalysts. The catalysts currently available for the production of terephthalic acid-based polyesters include antimony catalysts, tin catalysts, rare earth catalysts, and titanium catalysts. Antimony catalysts are cheap, but have low activity, and they often contain arsenic, making them highly toxic; tin catalysts are highly neurotoxic, highly irritating to the eyes and skin, and harmful to the environment, easily causing water pollution; rare earth catalysts are highly active, but expensive and not suitable for industrial applications; titanium catalysts are highly active, cheap, and have good ecological safety. At present, titanium catalysts are commonly used in industrial production. Titanium catalysts have some inherent defects in the process of efficiently catalyzing the synthesis of terephthalic acid-based polyesters. First, while titanium catalysts catalyze the condensation reaction of terephthalic acid-based polyesters, they also catalyze the thermal degradation reaction of terephthalic acid-based polyesters, making it difficult to increase the viscosity of terephthalic acid-based polyesters; second, titanium catalysts themselves will also undergo side reactions during the catalytic process to generate yellow substances, which will cause the hue of terephthalic acid-based polyesters to deteriorate. Summary of the invention
[0004] In view of this, the present application provides a modified titanium catalyst and a preparation method and application thereof, which solves the technical problem in the prior art that titanium catalysts will catalyze the thermal degradation reaction of terephthalic acid-based polyester while catalyzing the condensation reaction of terephthalic acid-based polyester, thereby making it difficult to increase the viscosity of terephthalic acid-based polyester. In addition, side reactions will also occur during the catalytic process, thereby causing the hue of the terephthalic acid-based polyester to deteriorate.
[0005] According to the first aspect of the present application, the present application provides a modified titanium catalyst, the general structural formula of the catalyst is:
[0006]
[0007] In the formula, R1 is an alkylene group having 1 to 7 carbon atoms, M includes a first coordination metal and a second coordination metal, the first coordination metal is cobalt, and the second coordination metal is at least one of zinc, manganese, nickel, and magnesium.
[0008] According to the second aspect of the present application, the present application provides a method for preparing a modified titanium catalyst, and the preparation of the catalyst includes the following steps: step S1, under the protection of an inert atmosphere gas, dripping an organic titanate in a certain proportion into a mixed solution of a hydroxy fatty acid and a saturated monohydric alcohol, stirring and reacting, and reacting at 60 to 110°C for 0.5 to 5 hours to obtain a catalyst precursor suspension; step S2, dispersing cobalt acetate and a second metal acetate in a saturated monohydric alcohol, and under the protection of an inert atmosphere gas, stirring and dripping the catalyst precursor suspension obtained in step S1, reacting at 60 to 110°C for 2 to 5 hours to obtain a catalyst suspension; step S3, centrifuging, washing, and drying the catalyst suspension obtained in step S2 to obtain the modified titanium catalyst described above.
[0009] In one embodiment, in step S2, the second metal acetate includes at least one of zinc acetate, magnesium acetate, nickel acetate, and manganese acetate; the molar ratio of the added amount of the cobalt acetate and the second metal acetate is 1:0.5-2; preferably, the molar ratio of the total added molar amount of the cobalt acetate and the second metal acetate to the added amount of the organic phthalate is 2-3:1.
[0010] In one embodiment, in step S1, the molar ratio of the organic phthalate, the hydroxy fatty acid and the saturated monohydric alcohol is 1:(1.01-1.1):(8-18); the organic titanate is a titanium compound having Ti(OR)4; and / or the hydroxy fatty acid is a hydroxy fatty acid having 2-8 carbon atoms and only one hydroxyl group and one carboxyl group.
[0011] In one embodiment, in step S1, the organic titanate is any one or more of tetraethyl titanate, tetraisopropyl titanate, tetra-n-propyl titanate, and tetra-n-butyl titanate; and / or the hydroxy fatty acid is any one or more of glycolic acid, 3-hydroxypropionic acid, lactic acid, and 4-hydroxybutyric acid.
[0012] In one embodiment, the saturated monohydric alcohols in step S1 and step S2 are both saturated monohydric alcohols having 2 to 10 carbon atoms.
[0013] In one embodiment, the saturated monohydric alcohol is any one or more of ethanol, isopropanol, propanol, and n-butanol.
[0014] According to the third aspect of the present application, the present application provides a method for preparing terephthalic acid-based polyester, using terephthalic acid and diol as raw monomers, and preparing poly(trimethylene terephthalate) after esterification reaction, pre-polycondensation reaction and final polycondensation reaction under the action of a modified titanium catalyst and a stabilizer; wherein the modified titanium catalyst is prepared by the preparation method of the modified titanium catalyst described above.
[0015] In one embodiment, the amount of the modified titanium catalyst is 500 to 2000 ppm of the total mass of the terephthalic acid and the diol; and / or, the molar ratio of the monomer diol and the terephthalic acid is 1.4 to 2:1; and / or, the amount of the stabilizer added is 50 to 250 ppm of the total mass of the terephthalic acid and the diol.
[0016] In one embodiment, the stabilizer includes one or more of triphenyl phosphate, triphenyl phosphite, triethyl phosphate, trimethyl phosphite, triethyl phosphite, triisopropyl phosphite, tri-tolyl phosphite, dimethyl phosphate, trimethyl phosphate, and diphenyl phosphate; and / or, the diol is one or more of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and 1,4-cyclohexanedimethanol; the esterification reaction conditions are: at a temperature of 200-240° C., a pressure of 100-400 KPaA, and a stirring rate of 1.5-2.0 %; Preferably, the pre-polycondensation reaction conditions are: at a temperature of 220 to 260° C., a pressure of 1 to 10 KPaA, and a stirring rate of 50 to 200 rpm, the pre-polycondensation reaction is carried out for 0.5 to 2 hours to obtain a polyterephthalic acid-based polyester prepolymer; preferably, the final polycondensation reaction conditions are: at a temperature of 240 to 300° C., a vacuum degree of 20 to 100 Pa, and a stirring rate of 50 to 200 rpm, the pre-polycondensation reaction is carried out for 0.2 to 1 hour to obtain a polyterephthalic acid-based polyester.
[0017] The present application provides a modified titanium catalyst and a preparation method and application thereof. Under the protection of an inert atmosphere gas, an organic titanate is dripped into a mixed solution of a hydroxy fatty acid and a saturated monohydric alcohol in a certain proportion, reacted while stirring, and reacted at 60-110° C. for 0.5-5 hours to obtain a catalyst precursor suspension; cobalt acetate and a second metal acetate are dispersed in a saturated monohydric alcohol, and under the protection of an inert atmosphere gas, the catalyst precursor suspension is dripped into the mixed solution while stirring, and reacted at 60-110° C. for 2-5 hours to obtain a catalyst suspension, and the catalyst suspension is centrifuged, washed, and dried to obtain a modified titanium catalyst. In the preparation process of the modified titanium catalyst, cobalt acetate and zinc acetate are used simultaneously, and the coordinated metal M itself has a certain effect on the polymerization reaction of polyester. The effect of the chemical activity can improve the catalytic efficiency to a certain extent. The second coordination metal (zinc, manganese, nickel, magnesium) plays a role of a catalyst promoter, which can increase the electron density of the Ti atom through the Ti-O-M bond bridge and thus affect the catalytic activity. In addition, the double titanium ring structure of the modified catalyst makes it more stable to resist the attack of hydrogen bonds and hydroxyl groups in water molecules, inhibiting the main chain structure of the polyester from breaking and decreasing the viscosity due to rearrangement reaction, but does not affect the chelate coordination between it and the oligomer molecular chain, so that it can achieve the catalytic activity of esterification and polycondensation while reducing the catalytic activity of thermal degradation of polyester, and taking into account the hue index at the same time. The modified titanium catalyst can not only ensure the reaction efficiency of the preparation of terephthalic acid-based polyester, but also effectively improve the hue of terephthalic acid-based polyester products. DETAILED DESCRIPTION
[0018] Mentioning "embodiment" in this article means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It will be understood by those skilled in the art that the embodiments described herein may be combined with other embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians of this field without making creative work are within the scope of protection of this application.
[0019] Unless otherwise specified, all reagents used in this application are commercially available.
[0020] In this application, the intrinsic viscosity of PET / PCT is tested with reference to the method of GB / T 14190-2008 Test method for fiber-grade polyester chips (PET), the solvent is phenol / 1,1,2,2-tetrachloroethane (mass ratio 50:50), and the Ubbelohde capillary viscometer is numbered 4-0.8.
[0021] The intrinsic viscosity of PTT was tested according to the method described in FZ / T 51010-2014 Fiber-grade poly(trimethylene terephthalate (PTT)). The solvent was phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40), and the Ubbelohde capillary viscometer number was 4-0.8.
[0022] The intrinsic viscosity of PBT was tested according to the method of "HG / T 5510-2019 Plastic Polybutylene Terephthalate (PBT) Resin". The solvent was phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40), and the Ubbelohde capillary viscometer number was 4-0.8.
[0023] The color values of PET / PCT / PTT / PBT all use the L, a, b color system as the evaluation benchmark. In this system, L is the brightness factor, and a and b are color measurement numbers. Among them, b represents the yellow-blue balance, which is very important for the color of polyester. The closer the b value is to 0, the better the color.
[0024] Example 1
[0025] Preparation of Catalyst I:
[0026] Step S1, 1.01 mol of glycolic acid and 8 mol of butanol are prepared into a mixed solution, and then 1 mol of tetra-n-butyl titanate is slowly dripped into the mixed solution under nitrogen protection and stirring conditions, and reacted at 110° C. for 0.5 h to obtain a catalyst precursor suspension;
[0027] Step S2, dispersing 1.34 mol of cobalt acetate and 0.67 mol of zinc acetate in n-butanol, slowly dripping into the catalyst precursor suspension of step S1 under nitrogen protection and stirring, and reacting at 110° C. for 2 h to obtain a catalyst suspension.
[0028] Step S3, centrifuging, washing and drying the catalyst suspension obtained in step S2 to obtain catalyst I.
[0029] Synthesis of polyethylene terephthalate (PET):
[0030] (1) Add the raw materials terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 into a polymerization reactor, and then add the catalyst I prepared above, the amount of catalyst I added is 2000ppm of the total mass of terephthalic acid and ethylene glycol. The atmosphere in the polymerization reactor is replaced with nitrogen to carry out esterification reaction, the temperature of the esterification reaction is 240°C, the pressure of the esterification reaction is 400KPaA, the stirring speed of the polymerization reactor is 200rpm, and the water output of the reaction system is recorded every 0.1h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid. The esterification reaction takes a total of 2h.
[0031] (2) Add 250 ppm of the stabilizer triphenyl phosphate to the reaction system obtained in step (1), and control the reaction system temperature to 260° C., the reaction system pressure to 10 kPaA, and the stirring speed to 200 rpm to perform a precondensation reaction to obtain a polyethylene terephthalate prepolymer, wherein the precondensation reaction lasts for 0.5 h.
[0032] (3) The polyethylene terephthalate prepolymer obtained in step (2) enters the final polycondensation reaction stage, the reaction system temperature is controlled to 260° C., the reaction system vacuum degree is 100 Pa, the stirring speed is 200 rpm, and the final polycondensation reaction is carried out. After the reaction is continued for 0.2 h, the reaction is stopped, the material is discharged and granulated, and the polyethylene terephthalate product can be obtained.
[0033] The intrinsic viscosity of polyethylene terephthalate synthesized by using this catalyst was 0.986 dL / g, and the b value was 2.8.
[0034] Example 2
[0035] Preparation of Catalyst II:
[0036] Step S1, 1.1 mol of lactic acid and 8 mol of butanol are prepared into a mixed solution, and then 1 mol of tetraethyl titanate is slowly dripped into the mixed solution under nitrogen protection and stirring conditions, and reacted at 60° C. for 5 hours to obtain a catalyst precursor suspension;
[0037] Step S2, dispersing 1 mol of cobalt acetate and 2 mol of magnesium acetate in n-butanol, slowly dripping into the catalyst precursor suspension of step S1 under nitrogen protection and stirring conditions, and reacting at 60° C. for 5 hours to obtain a catalyst suspension.
[0038] Step S3, centrifuging, washing and drying the catalyst suspension obtained in step S2 to obtain catalyst II.
[0039] Synthesis of polybutylene terephthalate (PBT):
[0040] (1) Add the raw materials terephthalic acid and 1,4-butanediol into a polymerization reactor in a molar ratio of 1:2, and then add the catalyst II prepared above, the amount of catalyst II added is 500ppm of the total mass of terephthalic acid and 1,4-butanediol. The atmosphere in the polymerization reactor is replaced with nitrogen to carry out esterification reaction, the temperature of the esterification reaction is 200°C, the pressure of the esterification reaction is 300KPaA, the stirring speed of the polymerization reactor is 50rpm, and the water output of the reaction system is recorded every 0.1h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid. The esterification reaction takes a total of 4h.
[0041] (2) Add 250 ppm of triphenyl phosphite as a stabilizer to the reaction system obtained in step (1), and control the reaction system temperature to 220° C., the reaction system pressure to 1 KPaA, and the stirring speed to 50 rpm to carry out a pre-polycondensation reaction to obtain a polybutylene terephthalate prepolymer, wherein the pre-polycondensation reaction lasts for 2 hours.
[0042] (3) The polybutylene terephthalate prepolymer obtained in step (2) enters the final polycondensation reaction stage, the reaction system temperature is controlled to 240° C., the reaction system vacuum degree is 20 Pa, the stirring speed is 50 rpm, and the final polycondensation reaction is carried out. After the reaction is continued for 1 hour, the reaction is stopped, the material is discharged and granulated, and the polybutylene terephthalate product can be obtained.
[0043] The intrinsic viscosity of polybutylene terephthalate synthesized by using this catalyst was 1.011 dL / g, and the b value was 2.2.
[0044] Example 3
[0045] Preparation of Catalyst III:
[0046] Step S1, 1.03 mol of hydroxypropionic acid and 10 mol of isopropanol are prepared into a mixed solution, and then 1 mol of tetraisopropyl titanate is slowly dripped into the mixed solution under nitrogen protection and stirring conditions, and reacted at 75° C. for 3.5 hours to obtain a catalyst precursor suspension;
[0047] Step S2, dispersing 1.2 mol of cobalt acetate and 1.2 mol of manganese acetate in isopropanol, slowly dripping into the catalyst precursor suspension of step S1 under nitrogen protection and stirring, and reacting at 70° C. for 4.5 hours to obtain a catalyst suspension.
[0048] Step S3, centrifuging, washing and drying the catalyst suspension obtained in step S2 to obtain catalyst III.
[0049] Synthesis of polytrimethylene terephthalate:
[0050] (1) Add the raw materials terephthalic acid and 1,3-propylene glycol in a molar ratio of 1:1.5 into a polymerization reactor, and then add the catalyst III prepared above, the amount of catalyst III added is 1000ppm of the total mass of terephthalic acid and 1,3-propylene glycol. The atmosphere in the polymerization reactor is replaced with nitrogen and then an esterification reaction is carried out. The temperature of the esterification reaction is 220°C, the pressure of the esterification reaction is 150KPaA, the stirring speed of the polymerization reactor is 100rpm, and the water output of the reaction system is recorded every 0.1h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid. The esterification reaction takes a total of 3h.
[0051] (2) Add 100 ppm of stabilizer triethyl phosphate to the reaction system obtained in step (1), and control the reaction system temperature to 250° C., the reaction system pressure to 4 kPaA, and the stirring speed to 100 rpm to perform a precondensation reaction to obtain a polytrimethylene terephthalate prepolymer, wherein the precondensation reaction lasts for 1 hour.
[0052] (3) The poly(trimethylene terephthalate) prepolymer obtained in step (2) enters the final polycondensation reaction stage, the reaction system temperature is controlled to be 250° C., the reaction system vacuum degree is 50 Pa, the stirring speed is 100 rpm, and the final polycondensation reaction is carried out. After the reaction is continued for 0.5 h, the reaction is stopped, the material is discharged and granulated, and the poly(trimethylene terephthalate) product is obtained.
[0053] The intrinsic viscosity of polytrimethylene terephthalate synthesized by using this catalyst was 1.035 dL / g, and the b value was 2.5.
[0054] Example 4
[0055] Preparation of Catalyst IV:
[0056] Step S1, 1.06 mol of hydroxybutyric acid and 14 mol of n-propanol are prepared into a mixed solution, and then 1 mol of tetra-n-propyl titanate is slowly dripped into the mixed solution under nitrogen protection and stirring conditions, and reacted at 90° C. for 2 hours to obtain a catalyst precursor suspension;
[0057] Step S2, dispersing 1.3 mol of cobalt acetate and 1.3 mol of nickel acetate in n-propanol, slowly dripping into the catalyst precursor suspension of step S1 under nitrogen protection and stirring conditions, and reacting at 90° C. for 3.5 hours to obtain a catalyst suspension.
[0058] Step S3, centrifuging, washing and drying the catalyst suspension obtained in step S2 to obtain catalyst IV.
[0059] Synthesis of polytrimethylene terephthalate (PTT):
[0060] (1) Add the raw materials terephthalic acid and 1,3-propylene glycol in a molar ratio of 1:1.7 to a polymerization reactor, and then add the catalyst IV prepared above, the amount of catalyst IV added is 1500ppm of the total mass of terephthalic acid and 1,3-propylene glycol. The atmosphere in the polymerization reactor is replaced with nitrogen and then an esterification reaction is carried out. The temperature of the esterification reaction is 230°C, the pressure of the esterification reaction is 400KPaA, the stirring speed of the polymerization reactor is 150rpm, and the water output of the reaction system is recorded every 0.1h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid. The esterification reaction takes a total of 3.5h.
[0061] (2) Add 100 ppm of triphenyl phosphite as a stabilizer to the reaction system obtained in step (1), and control the reaction system temperature to 240° C., the reaction system pressure to 17 kPaA, and the stirring speed to 150 rpm to carry out a precondensation reaction to obtain a polytrimethylene terephthalate prepolymer, wherein the precondensation reaction lasts for 1.5 hours.
[0062] (3) The poly(trimethylene terephthalate) prepolymer obtained in step (2) enters the final polycondensation reaction stage, the reaction system temperature is controlled to 260° C., the reaction system vacuum degree is 70 Pa, the stirring speed is 150 rpm, and the final polycondensation reaction is carried out. After the reaction is carried out for 0.6 h, the reaction is stopped, the material is discharged and granulated, and the poly(trimethylene terephthalate) product is obtained.
[0063] The intrinsic viscosity of polytrimethylene terephthalate synthesized by using this catalyst was 1.028 dL / g, and the b value was 2.4.
[0064] Example 5
[0065] Preparation of Catalyst I:
[0066] Step S1, 1.01 mol of glycolic acid and 8 mol of butanol are prepared into a mixed solution, and then 1 mol of tetra-n-butyl titanate is slowly dripped into the mixed solution under nitrogen protection and stirring conditions, and reacted at 110° C. for 0.5 h to obtain a catalyst precursor suspension;
[0067] Step S2, dispersing 1.34 mol of cobalt acetate and 0.67 mol of zinc acetate in n-butanol, slowly dripping into the catalyst precursor suspension of step S1 under nitrogen protection and stirring, and reacting at 110° C. for 2 h to obtain a catalyst suspension.
[0068] Step S3, centrifuging, washing and drying the catalyst suspension obtained in step S2 to obtain catalyst I.
[0069] Synthesis of poly(1,4-cyclohexanedimethanol terephthalate) (PCT):
[0070] (1) Add the raw materials terephthalic acid and 1,4-cyclohexanedimethanol into a polymerization reactor at a molar ratio of 1:1.8, and then add the catalyst I prepared above, the amount of catalyst I added is 1000ppm of the total mass of terephthalic acid and 1,4-cyclohexanedimethanol. The atmosphere in the polymerization reactor is replaced with nitrogen to carry out esterification reaction, the temperature of the esterification reaction is 240°C, the pressure of the esterification reaction is 100KPaA, the stirring speed of the polymerization reactor is 120rpm, and the water output of the reaction system is recorded every 0.1h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid. The esterification reaction takes a total of 3h.
[0071] (2) Add 350 ppm of the stabilizer triphenyl phosphate to the reaction system obtained in step (1), and control the reaction system temperature to 260° C., the reaction system pressure to 5 kPaA, and the stirring speed to 120 rpm to perform a precondensation reaction to obtain a poly(1,4-cyclohexanedimethanol terephthalate) prepolymer, wherein the precondensation reaction lasts for 0.8 h.
[0072] (3) The poly(1,4-cyclohexanedimethanol terephthalate) prepolymer obtained in step (2) is subjected to a final polycondensation reaction stage, the reaction system temperature is controlled to be 300° C., the reaction system vacuum degree is 80 Pa, the stirring speed is 120 rpm, and a final polycondensation reaction is carried out. After the reaction is carried out for 0.2 h, the reaction is stopped, the material is discharged and granulated, and a poly(1,4-cyclohexanedimethanol terephthalate) product is obtained.
[0073] The intrinsic viscosity of poly(1,4-cyclohexanedimethylene terephthalate) synthesized by using the catalyst I was 0.985 dL / g and the b value was 0.9.
[0074] Comparative Example 1
[0075] Compared with Example 1, during the catalyst preparation process, cobalt acetate was replaced with an equimolar amount of zinc acetate, and the other conditions remained unchanged.
[0076] Preparation of Catalyst V:
[0077] Step S1, 1.01 mol of glycolic acid and 8 mol of butanol are prepared into a mixed solution, and then 1 mol of tetra-n-butyl titanate is slowly dripped into the mixed solution under nitrogen protection and stirring conditions, and reacted at 110° C. for 0.5 h to obtain a catalyst precursor suspension;
[0078] Step S2, dispersing 2.01 mol of zinc acetate in n-butanol, slowly dripping it into the catalyst precursor suspension of step S1 under nitrogen protection and stirring, and reacting at 110° C. for 2 h to obtain a catalyst suspension.
[0079] Step S3, centrifuging, washing and drying the catalyst suspension obtained in step S2 to obtain catalyst V.
[0080] Synthesis of polyethylene terephthalate (PET):
[0081] (1) Add the raw materials terephthalic acid and ethylene glycol in a molar ratio of 1:1.4 into a polymerization reactor, and then add the catalyst V prepared above, the amount of catalyst V added is 2000ppm of the total mass of terephthalic acid and ethylene glycol. The atmosphere in the polymerization reactor is replaced with nitrogen and then an esterification reaction is carried out. The temperature of the esterification reaction is 240°C, the pressure of the esterification reaction is 200KPaA, the stirring speed of the polymerization reactor is 200rpm, and the water output of the reaction system is recorded every 0.1h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid. The esterification reaction takes a total of 2h.
[0082] (2) Add 250 ppm of the stabilizer triphenyl phosphate to the reaction system obtained in step (1), and control the reaction system temperature to 260° C., the reaction system pressure to 10 KPaA, and the stirring speed to 200 rpm to perform a precondensation reaction to obtain a polytrimethylene terephthalate prepolymer, wherein the precondensation reaction lasts for 0.5 h.
[0083] (3) The poly(trimethylene terephthalate) prepolymer obtained in step (2) is subjected to a final polycondensation reaction, wherein the temperature of the reaction system is controlled to be 280° C., the vacuum degree of the reaction system is controlled to be 100 Pa, and the stirring speed is controlled to be 200 rpm, and a final polycondensation reaction is carried out. After the reaction is carried out for 0.2 h, the reaction is stopped, the material is discharged and granulated, and a polyethylene terephthalate product is obtained.
[0084] The intrinsic viscosity of polyethylene terephthalate synthesized by using this catalyst was 0.997 dL / g, and the b value was 6.8.
[0085] Comparative Example 2
[0086] Compared with Example 2, magnesium acetate was replaced with an equimolar amount of cobalt acetate during the catalyst preparation process, and the other conditions remained unchanged.
[0087] Preparation of Catalyst VI:
[0088] Step S1, 1.1 mol of lactic acid and 8 mol of butanol are prepared into a mixed solution, and then 1 mol of tetraethyl titanate is slowly dripped into the mixed solution under nitrogen protection and stirring conditions, and reacted at 60° C. for 5 hours to obtain a catalyst precursor suspension;
[0089] Step S2, dispersing 3 mol of cobalt acetate in n-butanol, slowly dripping it into the catalyst precursor suspension of step S1 under nitrogen protection and stirring, and reacting at 60° C. for 5 hours to obtain a catalyst suspension.
[0090] Step S3, centrifuging, washing and drying the catalyst suspension obtained in step S2 to obtain catalyst VI.
[0091] Synthesis of polybutylene terephthalate (PBT):
[0092] (1) Add the raw materials terephthalic acid and 1,4-butanediol into a polymerization reactor in a molar ratio of 1:2, and then add the catalyst VI prepared above, the amount of catalyst VI added is 500ppm of the total mass of terephthalic acid and 1,4-butanediol. The atmosphere in the polymerization reactor is replaced with nitrogen to carry out esterification reaction, the temperature of the esterification reaction is 200°C, the pressure of the esterification reaction is 300KPaA, the stirring speed of the polymerization reactor is 50rpm, and the water output of the reaction system is recorded every 0.1h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid. The esterification reaction takes a total of 4h.
[0093] (2) Add 250 ppm of triphenyl phosphite as a stabilizer to the reaction system obtained in step (1), and control the reaction system temperature to 220° C., the reaction system pressure to 1 KPaA, and the stirring speed to 50 rpm to carry out a pre-polycondensation reaction to obtain a polybutylene terephthalate prepolymer, wherein the pre-polycondensation reaction lasts for 2 hours.
[0094] (3) The polybutylene terephthalate prepolymer obtained in step (2) enters the final polycondensation reaction stage, the reaction system temperature is controlled to 240° C., the reaction system vacuum degree is 20 Pa, the stirring speed is 50 rpm, and the final polycondensation reaction is carried out. After the reaction is continued for 1 hour, the reaction is stopped, the material is discharged and granulated, and the polybutylene terephthalate product can be obtained.
[0095] The intrinsic viscosity of polybutylene terephthalate synthesized by using this catalyst was 0.896 dL / g, and the b value was 2.2.
[0096] Comparative Example 3
[0097] Compared with Example 3, no acetate was added during the catalyst preparation process, and other conditions remained the same.
[0098] Preparation of catalyst:
[0099] Step S1, 1.03 mol of hydroxypropionic acid and 10 mol of isopropanol are prepared into a mixed solution, and then 1 mol of tetraisopropyl titanate is slowly dripped into the mixed solution under nitrogen protection and stirring conditions, and reacted at 75° C. for 3.5 hours to obtain a catalyst precursor suspension;
[0100] Step S2: centrifuge, wash and dry the catalyst precursor suspension obtained in step S1 to obtain catalyst VII.
[0101] Synthesis of polytrimethylene terephthalate:
[0102] (1) Add the raw monomers terephthalic acid and 1,3-propylene glycol into a polymerization reactor at a molar ratio of 1:1.5, and then add the catalyst VII prepared above, the amount of catalyst VII added is 1000ppm of the total mass of terephthalic acid and 1,3-propylene glycol. The atmosphere in the polymerization reactor is replaced with nitrogen and then an esterification reaction is carried out. The temperature of the esterification reaction is 220°C, the pressure of the esterification reaction is 150KPaA, the stirring speed of the polymerization reactor is 100rpm, and the water output of the reaction system is recorded every 0.1h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid. The esterification reaction takes a total of 3.3h.
[0103] (2) Add 100 ppm of stabilizer triethyl phosphate to the reaction system obtained in step (1), and control the reaction system temperature to 250° C., the reaction system pressure to 4 kPaA, and the stirring speed to 100 rpm to perform a precondensation reaction to obtain a polytrimethylene terephthalate prepolymer, wherein the precondensation reaction lasts for 1 hour.
[0104] (3) The poly(trimethylene terephthalate) prepolymer obtained in step (2) enters the final polycondensation reaction stage, the reaction system temperature is controlled to be 250° C., the reaction system vacuum degree is 50 Pa, the stirring speed is 100 rpm, and the final polycondensation reaction is carried out. After the reaction is continued for 0.5 h, the reaction is stopped, the material is discharged and granulated, and the poly(trimethylene terephthalate) product is obtained.
[0105] The intrinsic viscosity of polytrimethylene terephthalate synthesized by using this catalyst was 0.842 dL / g, and the b value was 8.3.
[0106] Comparative Example 4
[0107] Compared with Example 4, the catalyst was changed to tetraisopropyl titanate of the same mass, and the other conditions remained unchanged.
[0108] Synthesis of polytrimethylene terephthalate:
[0109] (1) Add the raw materials terephthalic acid and 1,3-propylene glycol into a polymerization reactor at a molar ratio of 1:1.5, and then add the catalyst tetraisopropyl titanate, the amount of the catalyst added is 1000ppm of the total mass of terephthalic acid and 1,3-propylene glycol. The atmosphere in the polymerization reactor is replaced with nitrogen to carry out esterification reaction, the temperature of the esterification reaction is 220°C, the pressure of the esterification reaction is 150KPaA, the stirring speed of the polymerization reactor is 100rpm, and the water output of the reaction system is recorded every 0.1h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid. The esterification reaction takes a total of 3h.
[0110] (2) Add 100 ppm of stabilizer triethyl phosphate to the reaction system obtained in step (1), and control the reaction system temperature to 250° C., the reaction system pressure to 4 kPaA, and the stirring speed to 100 rpm to perform a precondensation reaction to obtain a polytrimethylene terephthalate prepolymer, wherein the precondensation reaction lasts for 1 hour.
[0111] (3) The poly(trimethylene terephthalate) prepolymer obtained in step (2) enters the final polycondensation reaction stage, the reaction system temperature is controlled to be 250° C., the reaction system vacuum degree is 50 Pa, the stirring speed is 100 rpm, and the final polycondensation reaction is carried out. After the reaction is continued for 0.5 h, the reaction is stopped, the material is discharged and granulated, and the poly(trimethylene terephthalate) product is obtained.
[0112] The intrinsic viscosity of polytrimethylene terephthalate synthesized by using this catalyst was 0.749 dL / g, and the b value was 12.5.
[0113] The above examples and comparative examples are summarized in Table 1.
[0114] Table 1 Comparison of results of embodiments and comparative examples
[0115]
[0116] In the preparation process of the catalyst of Example 1, cobalt acetate and zinc acetate are used simultaneously, so that the catalyst adopts a structure coordinated with cobalt, which can significantly improve the color of the product without affecting the activity of the catalyst. Therefore, the b value of the polyethylene terephthalate prepared by the catalyst of Example 1 is 2.8, while in the preparation process of the catalyst in Comparative Example 1, only zinc acetate is used without adding cobalt acetate, and the b value of the polyethylene terephthalate prepared is 6.8; it can be seen that the catalyst of Example 1 can significantly improve the color of the polyester product without affecting the activity of the catalyst because it adopts a structure coordinated with cobalt.
[0117] In the preparation process of the catalyst of Example 2, cobalt acetate and magnesium acetate were used simultaneously, and the intrinsic viscosity of the obtained product was 1.011 dL / g; in the preparation process of the catalyst of Comparative Example 2, only cobalt acetate was used without other acetates, and the intrinsic viscosity of the polybutylene terephthalate prepared by the catalyst was only 0.896 dL / g, which was significantly lower than the intrinsic viscosity of the polybutylene terephthalate prepared in Example 2. Therefore, the presence of coordination metals such as magnesium and zinc has a significant promoting effect on the catalytic activity of the catalyst, so that a product with a higher intrinsic viscosity can be obtained under the same process conditions.
[0118] It can be seen from Example 3 and Comparative Examples 3 and 4 that after the commonly used organic titanate catalyst is transformed into a catalyst containing a double titanium ring structure, its catalyst activity and hydrolysis resistance have been greatly improved, but there is still a certain gap in performance compared with the catalyst using cobalt and other metal atoms for coordination.
[0119] It can be seen that the modified titanium catalyst prepared by the present invention, the structural design of its coordination with cobalt can make the catalyst take into account the toner function, further optimize the hue of the polyester product, and the second coordination metal (zinc, manganese, nickel, magnesium) plays a role of co-catalysis, which can improve the electron density of Ti atoms through the Ti-O-M bond bridge and thus affect the catalytic activity. In addition, the coordination metal M itself also has the effect of improving the catalytic activity for the polymerization reaction of polyester, which can improve the catalytic efficiency to a certain extent, and the double titanium ring structure of the catalyst makes it have a more stable ability to resist the attack of hydrogen bonds and hydroxyl groups in water molecules, thereby improving its hydrolysis resistance. In addition, the double titanium ring structure of the catalyst will also inhibit the phenomenon that the main chain structure of the polyester is broken and the viscosity decreases due to the rearrangement reaction, but it does not affect the chelate coordination between it and the oligomer molecular chain, so that it can achieve the catalytic activity of reducing the thermal degradation of polyester while taking into account the esterification and polycondensation catalytic activity, and at the same time take into account the hue index, which can overcome the problem of low product characteristic viscosity and poor hue that are easy to occur in the existing titanium catalyst.
[0120] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.
Claims
1. A modified titanium catalyst, characterized in that: The general structural formula of the catalyst is: In the formula, R1 is an alkylene group having 1 to 7 carbon atoms, M includes a first coordination metal and a second coordination metal, the first coordination metal is cobalt, and the second coordination metal is at least one of zinc, manganese, nickel, and magnesium.
2. A method for preparing a modified titanium catalyst, characterized in that: The method comprises the following preparation steps: Step S1, under the protection of an inert atmosphere, drop an organic titanate in a certain proportion into a mixed solution of a hydroxy fatty acid and a saturated monohydric alcohol, react while stirring, and react at 60 to 110° C. for 0.5 to 5 hours to obtain a catalyst precursor suspension; Step S2, dispersing cobalt acetate and a second metal acetate in a saturated monohydric alcohol, and dripping the catalyst precursor suspension obtained in step S1 into the catalyst precursor suspension under the protection of an inert atmosphere while stirring, and reacting at 60 to 110° C. for 2 to 5 hours to obtain a catalyst suspension; Step S3, centrifuging, washing and drying the catalyst suspension obtained in step S2 to obtain the modified titanium catalyst according to claim 1.
3. The method for preparing a modified titanium catalyst according to claim 2, characterized in that: In step S2, the second metal acetate includes at least one of zinc acetate, magnesium acetate, nickel acetate, and manganese acetate; the molar ratio of the cobalt acetate to the second metal acetate is 1:0.5-2; Preferably, the molar ratio of the total added molar amount of the cobalt acetate and the second metal acetate to the added amount of the organic phthalate is 2 to 3:
1.
4. The method for preparing a modified titanium catalyst according to claim 2, characterized in that: In the step S1, the molar ratio of the organic phthalate, the hydroxy fatty acid and the saturated monohydric alcohol is 1:(1.01-1.1):(8-18); the organic titanate is a titanium compound having Ti(OR)4; And / or, the hydroxy fatty acid is a hydroxy fatty acid having 2 to 8 carbon atoms and having only one hydroxyl group and one carboxyl group.
5. The method for preparing a modified titanium catalyst according to claim 4, characterized in that: In step S1, the organic titanate is any one or more of tetraethyl titanate, tetraisopropyl titanate, tetra-n-propyl titanate, and tetra-n-butyl titanate; and / or the hydroxy fatty acid is any one or more of glycolic acid, 3-hydroxypropionic acid, lactic acid, and 4-hydroxybutyric acid.
6. The method for preparing a modified titanium catalyst according to claim 2, characterized in that: The saturated monohydric alcohols in step S1 and step S2 are both saturated monohydric alcohols having 2 to 10 carbon atoms.
7. The method for preparing a modified titanium catalyst according to claim 6, characterized in that: The saturated monohydric alcohol is any one or more of ethanol, isopropanol, propanol and n-butanol.
8. A method for preparing terephthalate-based polyester, characterized in that: With terephthalic acid and diol as raw monomers, under the action of the modified titanium catalyst and the stabilizer, after esterification reaction, pre-polycondensation reaction and final polycondensation reaction, terephthalic acid-based polyester is prepared; wherein the modified titanium catalyst is prepared by the preparation method of the modified titanium catalyst described in any one of claims 2-7.
9. The method for preparing terephthalate-based polyester according to claim 8, characterized in that: The amount of the modified titanium catalyst is 500 to 2000 ppm of the total mass of the terephthalic acid and the diol; And / or, the molar ratio of the diol to the terephthalic acid is 1.4 to 2:1; And / or, the stabilizer is added in an amount of 50 to 250 ppm based on the total mass of the terephthalic acid and the diol.
10. The method for preparing terephthalate-based polyester according to claim 8, characterized in that: The stabilizer includes one or more of triphenyl phosphate, triphenyl phosphite, triethyl phosphate, trimethyl phosphite, triethyl phosphite, triisopropyl phosphite, tri-meta-cresyl phosphite, dimethyl phosphate, trimethyl phosphate, and diphenyl phosphate; And / or, the diol is one or more of ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and 1,4-cyclohexanedimethanol; The esterification reaction conditions are: esterification for 2 to 4 hours at a temperature of 200 to 240° C., a pressure of 100 to 400 KPaA, and a stirring rate of 50 to 200 rpm, and the esterification reaction is terminated when the water output reaches 90% of the theoretical water output; Preferably, the pre-polycondensation reaction conditions are: pre-polycondensation for 0.5 to 2 hours at a temperature of 220 to 260° C., a pressure of 1 to 10 KPaA, and a stirring rate of 50 to 200 rpm to obtain a terephthalic acid-based polyester prepolymer; Preferably, the final polycondensation reaction conditions are: polycondensation for 0.2 to 1 h at a temperature of 240 to 300° C., a vacuum degree of 20 to 100 Pa, and a stirring rate of 50 to 200 rpm to obtain terephthalic acid-based polyester.