Preparation method of terephthalic acid polyester

By using the synergistic action of triflate and heteropolyacid catalysts in the preparation of terephthalate polyester, the generation of cyclic oligomers is reduced, and the end hydroxyl backbite in the melt state is solved The problem has improved the utilization rate of raw materials and product stability.

CN119019660APending Publication Date: 2024-11-26CHINA TIANCHEN ENGINEERING CORPORATION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411044105.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the terephthalate polyester prepared by the melt polymerization method will cause end hydroxyl backbiting in the melt state, resulting in waste of raw materials, high production costs and occurrence of during processing. Frost, white mist and other problems.

Method used

The esterification reaction is carried out by mixing terephthalic acid, diol and organic titanium catalyst, followed by adding trifluoromethanesulfonate catalyst and heteropolyacid catalyst for pre-polycondensation, and then adding phosphite antioxidants for pre-polycondensation. Polycondensation reduces the amount of cyclic oligomer generation.

Benefits of technology

It effectively reduces the amount of ring-shaped oligomers generated during polymerization, improves raw material utilization and product quality, avoids frost and white mist during processing, and the catalyst used is stable and cheap.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004973049880000131
    Figure BDA0004973049880000131
  • Figure BDA0004973049880000141
    Figure BDA0004973049880000141
Patent Text Reader

Abstract

The preparation method of the terephthalic acid-based polyester provided by the invention comprises the following preparation steps: step (a), mixing terephthalic acid, dihydric alcohol and an organic titanium catalyst according to a certain proportion, and carrying out esterification reaction at a certain temperature, pressure and stirring speed; step (b), adding a certain amount of a trifluoromethanesulfonate catalyst and a heteropolyacid catalyst into the esterification reaction liquid, and carrying out a pre-polycondensation reaction at a certain temperature, pressure and stirring speed to obtain a pre-polycondensation reaction liquid; and (c) adding a certain amount of phosphite antioxidant into the pre-polycondensation reaction solution, and carrying out post-polycondensation reaction at a certain temperature, pressure and stirring speed to obtain the product terephthalic acid polyester. The trifluoromethanesulfonate catalyst and the heteropolyacid catalyst are matched, so that the generation amount of a by-product cyclic oligomer in the polymerization process is greatly reduced, and the generation amount of the cyclic oligomer is less than 0.35 wt%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of preparation of terephthalic acid-based polyesters, and in particular to a method for preparing terephthalic acid-based polyesters. Background Art

[0002] Polyester is a general term for polymers obtained by polycondensation of dibasic acids and diols. Since its introduction, it has attracted widespread attention due to its advantages such as high strength, corrosion resistance, and strong plasticity. Today, polyester materials are not only widely used in traditional fields such as textile fibers, films, bottle containers, automobiles, and electronics, but also have outstanding performance in many emerging fields such as national defense science and technology, aerospace, and communications.

[0003] There are many types of polyester materials, among which polyesters with terephthalic acid as raw material and building unit account for an absolute proportion. This is not only because terephthalic acid raw materials are easy to obtain and low in cost, but also related to the excellent performance of its downstream materials. At present, terephthalic acid-based polyesters are mainly prepared by melt polymerization of terephthalic acid and diols. The polyester prepared by the melt polymerization method will undergo end hydroxyl backbiting in the melt state to undergo ester exchange reaction with the ester bond, further generating cyclic oligomers as impurities. For terephthalic acid-based polyesters, most cyclic oligomers account for about 2.5% to 3% of the mass fraction of the polymer. The presence of cyclic oligomers will have some adverse effects on the production and processing of terephthalic acid polyesters. On the one hand, the generation of cyclic oligomers causes a waste of raw materials and increases the cost of production; on the other hand, cyclic oligomers are easy to volatilize at high temperatures and are easily accumulated in polymerization or processing equipment, thereby affecting the production and processing of polymers. For example, high content of cyclic oligomers will form white frost on the spinneret holes during polyester spinning, causing spinneret blockage, flying and broken yarns, etc. Therefore, reducing the content of cyclic oligomers can not only reduce raw material consumption and save costs, but also help improve the appearance and performance of products, and reduce the phenomenon of frost and white foaming of polyester during spinning and injection molding, reduce the number of shutdowns for cleaning, and increase product output.

[0004] The invention patent with the publication number CN1211413C and the patent name "Method for producing poly(propylene terephthalate)" discloses a method of separating cyclic oligomers from the polymerization system and recycling them to the polymerization process after treatment, which effectively avoids the loss of raw materials. However, the recovery and application process of the cyclic oligomers is complicated and the cost is high. The invention patent with the publication number CN1984962A and the patent name "Poly(propylene terephthalate)" reduces the amount of cyclic oligomers generated in the polymer and the remelted polymer by adding phosphonates or phosphinic acid compounds, but the process can only directly obtain PTT products with low intrinsic viscosity. If the intrinsic viscosity of the product is to be increased, the product needs to be further solid-phase thickened. The publication number is CN107955149B, and the patent name is "Production Method of Polytrimethylene Terephthalate with Low Cyclic Oligomer Content". The production of cyclic oligomers in the PTT polymerization process is reduced by using a specially designed catalyst, but compared with conventional technology, it can only reduce the content of cyclic oligomers by about 50%, and the actual effect is not ideal. Summary of the invention

[0005] In view of this, the present application provides a method for preparing terephthalic acid-based polyester, which solves the technical problem that the polyester prepared by the melt polymerization method in the prior art will undergo end hydroxyl group backbiting in the melt state to undergo ester exchange reaction with the ester bond, further generating cyclic oligomers as impurities, and the high content of cyclic oligomers causes waste of raw materials and high production costs.

[0006] The present application provides a method for preparing a terephthalic acid-based ester, comprising the following preparation steps: step (a), mixing terephthalic acid, a diol and an organic titanium catalyst in a certain proportion, and performing an esterification reaction at a certain temperature, pressure and stirring speed to obtain an esterification reaction liquid; step (b), adding a certain amount of a trifluoromethanesulfonate catalyst and a heteropolyacid catalyst to the esterification reaction liquid obtained in step (a), and performing a pre-polycondensation reaction at a certain temperature, pressure and stirring speed to obtain a pre-polycondensation reaction liquid; step (c), adding a certain amount of a phosphite antioxidant to the pre-polycondensation reaction liquid obtained in step (b), and performing a post-polycondensation reaction at a certain temperature, pressure and stirring speed to obtain a product, a terephthalic acid-based polyester.

[0007] In one embodiment, in the step (a), the organic titanium catalyst includes one or more of ethylene glycol titanium, propylene glycol titanium, butanediol titanium, tetraethyl titanate, tetraisopropyl titanate, tetra-n-propyl titanate, and tetra-n-butyl titanate; the diol includes one of ethylene glycol, 1,3-propylene glycol, and 1,4-butanediol.

[0008] In one embodiment, in the step (a), the molar ratio of the added amount of terephthalic acid to the diol is 1:1.4-2.2, and the added amount of the organic titanium catalyst is 300-1500 ppm of the total mass of the terephthalic acid and the diol.

[0009] In one embodiment, in the step (a), the esterification reaction temperature is 200-240° C.; the esterification reaction pressure is 150-400 KPaA; the esterification reaction time is 2-4.5 h; the stirring speed is 50-200 rpm;

[0010] In one embodiment, in the step (b), the triflate catalyst comprises one or more of zinc triflate, scandium triflate, indium triflate, aluminum triflate, cerium triflate, and copper triflate; the amount of the triflate catalyst added is 50 to 250 ppm of the total mass of the terephthalic acid and the diol;

[0011] In one embodiment, in step (b), the heteropolyacid catalyst includes one or more of phosphotungstic acid, silicotungstic acid, phosphomolybdic acid, and silicomolybdic acid, and the added amount of the heteropolyacid catalyst is 50 to 250 ppm of the total mass of the terephthalic acid and the diol.

[0012] In one embodiment, in the step (b), the pre-polycondensation temperature is 220-260° C.; the pre-polycondensation pressure is 200-1000 PaA; the pre-polycondensation reaction time is 0.5-1.5 h; and the stirring speed is 50-200 rpm.

[0013] In one embodiment, in the step (c), the phosphite antioxidant includes one or more of tris(2,4-di-tert-butylphenyl)phosphite, bis[2-methyl-4,6-bis(1,1'-dimethylethyl)phenol]ethyl phosphate, tetrakis(2,4-di-tert-butyloctaalkoxy-4,4-biphenylyl)phosphate, pentaerythritol bis(2,4-tert-butylphenyl)diphosphite, (2,4,6-tri-tert-butylphenyl-2-butyl-2-ethyl)-1,3-propanediol phosphite, di(2,4-di-p-isopropylphenyl)pentaerythritol bisphosphite, 2,2'-ethylenebis(4,6-di-tert-butylphenyl)fluorophosphite, tetrakis(2,4-di-tert-butylphenyl-4,4-biphenylyl)bisphosphate, and spiroethylene glycol di[2,2'-methylenebis(4,6-di-tert-butylphenyl)]phosphite.

[0014] In one embodiment, in the step (c), the added amount of the phosphite antioxidant is 250 to 1000 ppm of the pre-condensation reaction liquid; the temperature of the post-condensation is 240 to 280°C; the vacuum degree of the post-condensation is 20 to 100 Pa; and the time of the post-condensation is 1 to 2.5 hours.

[0015] In one embodiment, the cyclic oligomer content of the prepared terephthalic acid-based polyester is less than 0.35wt%; the generation rate of the cyclic oligomers of the prepared terephthalic acid-based polyester is less than 0.16wt% / h; the intrinsic viscosity of the prepared terephthalic acid-based polyester is 0.996-1.073dL / g.

[0016] The present application provides a method for preparing a terephthalic acid-based polyester, comprising the following preparation steps: step (a), mixing terephthalic acid, a diol and an organic titanium catalyst in a certain proportion, and performing an esterification reaction at a certain temperature, pressure and stirring speed to obtain an esterification reaction liquid; step (b), adding a certain amount of a trifluoromethanesulfonate catalyst and a heteropolyacid catalyst to the esterification reaction liquid obtained in step (a), and performing a pre-polycondensation reaction at a certain temperature, pressure and stirring speed to obtain a pre-polycondensation reaction liquid; step (c), adding a certain amount of a phosphite antioxidant to the pre-polycondensation reaction liquid obtained in step (b), and performing a post-polycondensation reaction at a certain temperature, pressure and stirring speed to obtain a product terephthalic acid-based polyester. The present application can effectively open the ring structure of the cyclic oligomer generated in the polyester melt again and re-add it to the polycondensation process by combining the trifluoromethanesulfonate catalyst and the heteropolyacid catalyst. Under the synergistic effect of the trifluoromethanesulfonate catalyst and the heteropolyacid catalyst, the carbonyl group in the generated cyclic by-product is activated, which can facilitate the nucleophilic attack of the terminal hydroxyl group in the polyester, so that the ring structure of the generated cyclic by-product is opened and re-added to the polycondensation process, which greatly reduces the amount of by-product cyclic oligomers generated during the polymerization process, and the amount of cyclic oligomers generated is less than 0.35wt%. Moreover, even in the melt processing process, it is difficult for terephthalate esters to generate by-product cyclic oligomers, thereby avoiding the occurrence of "blooming" and "white fog" during the processing process, and significantly improving the utilization rate of raw materials and product quality. DETAILED DESCRIPTION

[0017] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments. Based on the embodiments in the present application, all other embodiments obtained by those of ordinary skill in the art without making creative efforts are within the scope of protection of the present application.

[0018] Unless otherwise specified, all reagents used in this application are commercially available.

[0019] Example 1

[0020] The preparation steps of polytrimethylene terephthalate with low cyclic oligomer content of Example 1 are as follows:

[0021] Step (a), adding raw materials terephthalic acid and 1,3-propylene glycol into a polymerization reactor in a molar ratio of 1:1.4, adding a catalyst tetra-n-butyl titanate in an amount of 1500ppm of the total mass of terephthalic acid and 1,3-propylene glycol, replacing the atmosphere in the polymerization reactor with nitrogen, and then carrying out an esterification reaction, the esterification reaction temperature is 240°C, the esterification reaction pressure is 400KPaA, the stirring speed of the polymerization reactor is 200rpm, recording the water output of the reaction system every 0.1h, and when the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid, and the esterification reaction is terminated in a total of 2h.

[0022] Step (b), adding 250 ppm of zinc trifluoromethanesulfonate and 50 ppm of phosphotungstic acid to the esterification reaction liquid obtained in step (a), controlling the temperature of the reaction system to 260° C., the pressure of the reaction system to 1000 PaA, and the stirring speed to 200 rpm, to carry out a pre-polycondensation reaction to obtain a pre-polycondensation reaction liquid (polytrimethylene terephthalate prepolymer), and the pre-polycondensation reaction lasts for 0.5 h.

[0023] Step (c), adding 1000ppm of tris(2,4-di-tert-butylphenyl)phosphite to the pre-polycondensation reaction liquid obtained in step (b), controlling the temperature of the reaction system to 280°C, the vacuum degree of the reaction system to 100Pa, the stirring speed to 200rpm, and carrying out a post-polycondensation reaction. After reacting for 1h, stopping the reaction, discharging and granulating, and obtaining a polytrimethylene terephthalate product.

[0024] The polytrimethylene terephthalate product prepared in this embodiment was subjected to a PTT intrinsic viscosity test. The intrinsic viscosity of the polytrimethylene terephthalate product was 0.996 dL / g. The PTT intrinsic viscosity was tested according to the method of "FZ / T 51010-2014 Fiber-grade poly(trimethylene terephthalate) (PTT)". The solvent was phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40), and the Ubbelohde capillary viscometer was numbered 4-0.8.

[0025] The cyclic oligomer content of the poly(trimethylene terephthalate) prepared in this embodiment can be obtained by liquid chromatography after Soxhlet extraction. The poly(trimethylene terephthalate) is extracted using CH2Cl2 as a solvent, and the cyclic oligomer content in the extract is analyzed by liquid chromatography and its content in the polymer is calculated. The content of cyclic oligomers in the poly(trimethylene terephthalate) is 0.31wt% after liquid chromatography testing and calculation.

[0026] The generation rate of cyclic oligomers of the poly(trimethylene terephthalate) prepared in this embodiment during the melt processing was tested. The testing method was to remelt the prepared poly(trimethylene terephthalate) in a nitrogen atmosphere at a temperature of 260° C. and maintain it for 0.5 h. Then, the cyclic oligomer content in the poly(trimethylene terephthalate) before and after remelting was analyzed, and the generation rate of the cyclic oligomers was calculated. After testing and calculation, the generation rate of cyclic oligomers in the poly(trimethylene terephthalate) was 0.16 wt% / h.

[0027] Example 2

[0028] The preparation steps of polytrimethylene terephthalate with low cyclic oligomer content of Example 2 are as follows:

[0029] Step (a), adding raw materials terephthalic acid and 1,3-propylene glycol into a polymerization reactor in a molar ratio of 1:2.2, and adding a catalyst tetrabutyl titanate in an amount of 300ppm of the total mass of terephthalic acid and 1,3-propylene glycol. The atmosphere in the polymerization reactor is replaced with nitrogen and then an esterification reaction is carried out. The temperature of the esterification reaction is 200°C, the pressure of the esterification reaction is 150KPaA, the stirring speed of the polymerization reactor is 50rpm, and the water output of the reaction system is recorded every 0.1h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid. The esterification reaction is terminated in a total of 4.5h.

[0030] Step (b), adding 50 ppm of aluminum trifluoromethanesulfonate and 250 ppm of phosphomolybdic acid to the esterification reaction liquid obtained in step (a), controlling the reaction system temperature to 220° C., the reaction system pressure to 200 PaA, and the stirring speed to 50 rpm, to carry out a pre-polycondensation reaction to obtain a pre-polycondensation reaction liquid (polytrimethylene terephthalate prepolymer), and the pre-polycondensation reaction lasts for 1.5 hours.

[0031] Step (c), adding 250ppm of (2,4,6-tri-tert-butylphenyl-2-butyl-2-ethyl)-1,3-propylene glycol phosphite to the pre-polycondensation reaction liquid obtained in step (b), controlling the temperature of the reaction system to 240°C, the vacuum degree of the reaction system to 20Pa, the stirring speed to 50rpm, and performing a post-polycondensation reaction. After reacting for 2.5h, stopping the reaction, discharging and granulating, and obtaining a poly(trimethylene terephthalate) product.

[0032] The polytrimethylene terephthalate product prepared in this embodiment was subjected to a PTT intrinsic viscosity test. The intrinsic viscosity of the polytrimethylene terephthalate product was 1.054 dL / g. The PTT intrinsic viscosity was tested according to the method of "FZ / T 51010-2014 Fiber-grade poly(trimethylene terephthalate) (PTT)". The solvent was phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40), and the Ubbelohde capillary viscometer was numbered 4-0.8.

[0033] The cyclic oligomer content of the poly(trimethylene terephthalate) prepared in this embodiment can be obtained by liquid chromatography after Soxhlet extraction. The poly(trimethylene terephthalate) is extracted using CH2Cl2 as a solvent, and the cyclic oligomer content in the extract is analyzed by liquid chromatography and its content in the polymer is calculated. The content of cyclic oligomers in the poly(trimethylene terephthalate) is 0.29wt% after liquid chromatography testing and calculation.

[0034] The generation rate of cyclic oligomers of the poly(trimethylene terephthalate) prepared in this embodiment during the melt processing was tested. The testing method was to remelt the prepared poly(trimethylene terephthalate) in a nitrogen atmosphere at a temperature of 260° C. and maintain it for 0.5 h. Then, the cyclic oligomer content in the poly(trimethylene terephthalate) before and after remelting was analyzed, and the generation rate of the cyclic oligomers was calculated. After testing and calculation, the generation rate of the cyclic oligomers in the poly(trimethylene terephthalate) was 0.14 wt% / h.

[0035] Example 3

[0036] The preparation steps of polytrimethylene terephthalate with low cyclic oligomer content of Example 3 are as follows:

[0037] Step (a), adding raw materials terephthalic acid and 1,3-propylene glycol into a polymerization reactor in a molar ratio of 1:1.7, adding a catalyst tetra-n-butyl titanate in an amount of 800 ppm of the total mass of terephthalic acid and 1,3-propylene glycol, replacing the atmosphere in the polymerization reactor with nitrogen and then performing an esterification reaction, the temperature of the esterification reaction is 220°C, the pressure of the esterification reaction is 350 KPaA, the stirring speed of the polymerization reactor is 100 rpm, recording the water output of the reaction system every 0.1 h, and when the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid, and the esterification reaction is terminated in a total of 3.5 h.

[0038] Step (b), adding 150 ppm of scandium trifluoromethanesulfonate and 150 ppm of silicomolybdic acid to the esterification reaction liquid obtained in step (a), controlling the temperature of the reaction system to 240° C., the pressure of the reaction system to 400 PaA, and the stirring speed to 100 rpm, to carry out a precondensation reaction to obtain a precondensation reaction liquid (polytrimethylene terephthalate prepolymer), and the precondensation reaction lasts for 1 hour.

[0039] Step (c), adding 500ppm of spiroethylene glycol di[2,2-methylenebis(4,6-di-tert-butylphenyl)]phosphite to the pre-polycondensation reaction liquid obtained in step (b), controlling the temperature of the reaction system to 260°C, the vacuum degree of the reaction system to 40Pa, the stirring speed to 100rpm, and carrying out a post-polycondensation reaction. After reacting for 1.5h, stopping the reaction, discharging and granulating, and obtaining a polytrimethylene terephthalate product.

[0040] The polytrimethylene terephthalate product prepared in this embodiment was subjected to a PTT intrinsic viscosity test. The intrinsic viscosity of the polytrimethylene terephthalate product was 1.038 dL / g. The PTT intrinsic viscosity was tested according to the method of "FZ / T 51010-2014 Fiber-grade poly(trimethylene terephthalate) (PTT)". The solvent was phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40), and the Ubbelohde capillary viscometer was numbered 4-0.8.

[0041] The cyclic oligomer content of the poly(trimethylene terephthalate) prepared in this embodiment can be obtained by liquid chromatography after Soxhlet extraction. The poly(trimethylene terephthalate) is extracted using CH2Cl2 as a solvent, and the cyclic oligomer content in the extract is analyzed by liquid chromatography and its content in the polymer is calculated. The content of cyclic oligomers in the poly(trimethylene terephthalate) is 0.32wt% after liquid chromatography testing and calculation.

[0042] The generation rate of cyclic oligomers of the poly(trimethylene terephthalate) prepared in this embodiment during the melt processing was tested. The testing method was to remelt the prepared poly(trimethylene terephthalate) in a nitrogen atmosphere at a temperature of 260° C. and maintain it for 0.5 h. Then, the cyclic oligomer content in the poly(trimethylene terephthalate) before and after remelting was analyzed, and the generation rate of the cyclic oligomers was calculated. After testing and calculation, the generation rate of the cyclic oligomers in the poly(trimethylene terephthalate) was 0.15 wt% / h.

[0043] Example 4

[0044] The preparation steps of polytrimethylene terephthalate with low cyclic oligomer content of Example 4 are as follows:

[0045] Step (a), adding raw materials terephthalic acid and 1,3-propylene glycol into a polymerization reactor in a molar ratio of 1:2, adding a catalyst tetra-n-butyl titanate in an amount of 1000 ppm of the total mass of terephthalic acid and 1,3-propylene glycol, replacing the atmosphere in the polymerization reactor with nitrogen, and then carrying out an esterification reaction at a temperature of 230° C., a pressure of 250 KPaA, and a stirring speed of 150 rpm for the polymerization reactor. The esterification reaction is carried out, and the water output of the reaction system is recorded every 0.1 h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid. The esterification reaction takes 2.5 h in total.

[0046] Step (b), adding 100 ppm of copper trifluoromethanesulfonate and 200 ppm of silicotungstic acid to the esterification reaction liquid obtained in step (a), controlling the temperature of the reaction system to 250° C., the pressure of the reaction system to 600 PaA, and the stirring speed to 100 rpm, to carry out a pre-polycondensation reaction to obtain a pre-polycondensation reaction liquid (polytrimethylene terephthalate prepolymer), and the pre-polycondensation reaction lasts for 1 hour.

[0047] Step (c), adding 750ppm of di(2,4-di-p-isopropylphenyl)pentaerythritol diphosphite to the pre-polycondensation reaction liquid obtained in step (b), controlling the temperature of the reaction system to 250°C, the vacuum degree of the reaction system to 60Pa, the stirring speed to 100rpm, and carrying out a post-polycondensation reaction. After reacting for 2h, stopping the reaction, discharging and granulating, and obtaining a poly(trimethylene terephthalate) product.

[0048] The polytrimethylene terephthalate product prepared in this embodiment was subjected to a PTT intrinsic viscosity test. The intrinsic viscosity of the polytrimethylene terephthalate product was 1.073 dL / g. The PTT intrinsic viscosity was tested according to the method of "FZ / T 51010-2014 Fiber-grade poly(1,3-trimethylene terephthalate (PTT)". The solvent was phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40), and the Ubbelohde capillary viscometer was numbered 4-0.8.

[0049] The cyclic oligomer content of the poly(trimethylene terephthalate) prepared in this embodiment can be obtained by liquid chromatography after Soxhlet extraction. The poly(trimethylene terephthalate) is extracted using CH2Cl2 as a solvent, and the cyclic oligomer content in the extract is analyzed by liquid chromatography and its content in the polymer is calculated. The content of cyclic oligomers in the poly(trimethylene terephthalate) is 0.35wt% after liquid chromatography testing and calculation.

[0050] The generation rate of cyclic oligomers of the poly(trimethylene terephthalate) prepared in this embodiment during the melt processing was tested. The testing method was to remelt the prepared poly(trimethylene terephthalate) in a nitrogen atmosphere at a temperature of 260° C. and maintain it for 0.5 h. Then, the cyclic oligomer content in the poly(trimethylene terephthalate) before and after remelting was analyzed, and the generation rate of the cyclic oligomers was calculated. After testing and calculation, the generation rate of the cyclic oligomers in the poly(trimethylene terephthalate) was 0.14 wt% / h.

[0051] Example 5

[0052] The preparation steps of the polyethylene terephthalate with low cyclic oligomer content of Example 5 are as follows:

[0053] Step (a), adding raw materials terephthalic acid and ethylene glycol in a molar ratio of 1:1.6 into a polymerization reactor, adding a catalyst tetra-n-butyl titanate in an amount of 1200ppm of the total mass of terephthalic acid and ethylene glycol, replacing the atmosphere in the polymerization reactor with nitrogen and then carrying out an esterification reaction, the esterification reaction temperature is 220°C, the esterification reaction pressure is 300KPaA, the stirring speed of the polymerization reactor is 180rpm, recording the water output of the reaction system every 0.1h, and when the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid, and the esterification reaction is terminated in a total time of 2.5h.

[0054] Step (b), adding 200 ppm of zinc trifluoromethanesulfonate and 150 ppm of phosphotungstic acid to the esterification reaction liquid obtained in step (a), controlling the temperature of the reaction system to 260° C., the pressure of the reaction system to 1000 PaA, and the stirring speed to 200 rpm, to carry out a pre-polycondensation reaction to obtain a pre-polycondensation reaction liquid (polyethylene terephthalate prepolymer), and the pre-polycondensation reaction lasts for 0.8 h.

[0055] Step (c), adding 1000ppm of tris(2,4-di-tert-butylphenyl)phosphite to the pre-polycondensation reaction liquid obtained in step (b), controlling the temperature of the reaction system to 280°C, the vacuum degree of the reaction system to 100Pa, the stirring speed to 200rpm, and carrying out a post-polycondensation reaction. After reacting for 1h, stopping the reaction, discharging and granulating, and obtaining a polyethylene terephthalate product.

[0056] The PET intrinsic viscosity of the polyethylene terephthalate product prepared in this embodiment was tested. The intrinsic viscosity of the polyethylene terephthalate product was 1.001 dL / g. The PET intrinsic viscosity was tested according to the method of "GB / T 14190-2008 Test method for fiber-grade polyester chips (PET)". The solvent was phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40), and the Ubbelohde capillary viscometer was numbered 4-0.8.

[0057] The cyclic oligomer content of the polyethylene terephthalate prepared in this embodiment can be obtained by liquid chromatography after Soxhlet extraction. Use CH2Cl2 as a solvent to extract polyethylene terephthalate, analyze the cyclic oligomer content in the extract by liquid chromatography and calculate its content in the polymer. The content of cyclic oligomers in the polyethylene terephthalate is 0.30wt% after liquid chromatography testing and calculation.

[0058] The generation rate of cyclic oligomers of the polyethylene terephthalate prepared in this embodiment during the melt processing was tested. The testing method was to remelt the prepared polyethylene terephthalate in a nitrogen atmosphere at a temperature of 280° C. and maintain it for 0.5 h. Then, the cyclic oligomer content in the polyethylene terephthalate before and after remelting was analyzed, and the generation rate of the cyclic oligomers was calculated. After testing and calculation, the generation rate of the cyclic oligomers in the polyethylene terephthalate was 0.14wt% / h.

[0059] Example 6

[0060] The preparation steps of the polybutylene terephthalate with low cyclic oligomer content of Example 6 are as follows:

[0061] Step (a), adding raw materials terephthalic acid and 1,4-butanediol into a polymerization reactor in a molar ratio of 1:1.9, adding a catalyst tetrabutyl titanate in an amount of 900 ppm of the total mass of terephthalic acid and 1,4-butanediol, and performing an esterification reaction after the atmosphere in the polymerization reactor is replaced by nitrogen, the temperature of the esterification reaction is 210° C., the pressure of the esterification reaction is 250 KPaA, the stirring speed of the polymerization reactor is 120 rpm, and the water output of the reaction system is recorded every 0.1 h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid, and the esterification reaction is terminated in a total time of 3.0 h.

[0062] Step (b), adding 180ppm of scandium trifluoromethanesulfonate and 120ppm of silicomolybdic acid to the esterification reaction liquid obtained in step (a), controlling the reaction system temperature to 240°C, the reaction system pressure to 400PaA, and the stirring speed to 120rpm, and performing a pre-polycondensation reaction to obtain a pre-polycondensation reaction liquid (polybutylene terephthalate prepolymer), and the pre-polycondensation reaction duration is 1.2h.

[0063] Step (c), adding 600ppm of spiroethylene glycol di[2,2-methylenebis(4,6-di-tert-butylphenyl)]phosphite to the pre-polycondensation reaction liquid obtained in step (b), controlling the temperature of the reaction system to 260°C, the vacuum degree of the reaction system to 50Pa, the stirring speed to 120rpm, and carrying out a post-polycondensation reaction. After reacting for 1.2h, stopping the reaction, discharging and granulating, and obtaining a polybutylene terephthalate product.

[0064] The polybutylene terephthalate product prepared in this embodiment was tested for its PBT intrinsic viscosity. The intrinsic viscosity of the polybutylene terephthalate product was 1.015 dL / g. The PBT intrinsic viscosity was tested according to the method of "HG / T 5510-2019 Plastic Polybutylene Terephthalate (PBT) Resin". The solvent was phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40), and the Ubbelohde capillary viscometer was numbered 4-0.8.

[0065] The cyclic oligomer content of the polybutylene terephthalate prepared in this embodiment can be obtained by liquid chromatography after Soxhlet extraction. Use CH2Cl2 as a solvent to extract polybutylene terephthalate, analyze the cyclic oligomer content in the extract by liquid chromatography and calculate its content in the polymer. The content of cyclic oligomers in the polybutylene terephthalate obtained by liquid chromatography and calculation is 0.33wt%.

[0066] The generation rate of cyclic oligomers of the polybutylene terephthalate prepared in this embodiment during the melt processing was tested. The testing method was to remelt the prepared polybutylene terephthalate in a nitrogen atmosphere at a temperature of 260° C. and maintain it for 0.5 h. Then, the cyclic oligomer content in the polybutylene terephthalate before and after remelting was analyzed, and the generation rate of the cyclic oligomers was calculated. After testing and calculation, the generation rate of the cyclic oligomers in the polybutylene terephthalate was 0.16wt% / h.

[0067] Comparative Example 1

[0068] The preparation steps of the polytrimethylene terephthalate with low cyclic oligomer content of Comparative Example 1 are as follows:

[0069] Step (a), adding raw materials terephthalic acid and 1,3-propylene glycol into a polymerization reactor in a molar ratio of 1:1.4, and adding a catalyst tetrabutyl titanate in an amount of 1500ppm of the total mass of terephthalic acid and 1,3-propylene glycol. The atmosphere in the polymerization reactor is replaced with nitrogen to carry out an esterification reaction, the temperature of the esterification reaction is 240°C, the pressure of the esterification reaction is 400KPaA, the stirring speed of the polymerization reactor is 200rpm, and the water output of the reaction system is recorded every 0.1h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid, and the esterification reaction is terminated in a total of 2h.

[0070] Step (b), adding 250 ppm of phosphotungstic acid to the esterification reaction liquid obtained in step (a), controlling the reaction system temperature to 260°C, the reaction system pressure to 1000 PaA, and the stirring speed to 200 rpm, and performing a pre-polycondensation reaction to obtain a pre-polycondensation reaction liquid (polytrimethylene terephthalate prepolymer), and the pre-polycondensation reaction duration is 0.5 h.

[0071] Step (c), adding 1000ppm of tris(2,4-di-tert-butylphenyl)phosphite to the pre-polycondensation reaction liquid obtained in step (b), controlling the temperature of the reaction system to 280°C, the vacuum degree of the reaction system to 100Pa, the stirring speed to 200rpm, and carrying out a post-polycondensation reaction. After reacting for 1h, stopping the reaction, discharging and granulating, and obtaining a polytrimethylene terephthalate product.

[0072] The polytrimethylene terephthalate product prepared in this embodiment was subjected to a PTT intrinsic viscosity test. The intrinsic viscosity of the polytrimethylene terephthalate product was 0.895 dL / g. The PTT intrinsic viscosity was tested according to the method of "FZ / T 51010-2014 Fiber-grade poly(trimethylene terephthalate) (PTT)". The solvent was phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40), and the Ubbelohde capillary viscometer was numbered 4-0.8.

[0073] The cyclic oligomer content of the poly(trimethylene terephthalate) prepared in this embodiment can be obtained by liquid chromatography after Soxhlet extraction. The poly(trimethylene terephthalate) is extracted using CH2Cl2 as a solvent, and the cyclic oligomer content in the extract is analyzed by liquid chromatography and its content in the polymer is calculated. The content of cyclic oligomers in the poly(trimethylene terephthalate) is 1.83wt% after liquid chromatography testing and calculation.

[0074] The generation rate of cyclic oligomers of the poly(trimethylene terephthalate) prepared in this embodiment during the melt processing was tested. The testing method was to remelt the prepared poly(trimethylene terephthalate) in a nitrogen atmosphere at a temperature of 260° C. and maintain it for 0.5 h. Then, the cyclic oligomer content in the poly(trimethylene terephthalate) before and after remelting was analyzed, and the generation rate of the cyclic oligomers was calculated. After testing and calculation, the generation rate of the cyclic oligomers in the poly(trimethylene terephthalate) was 1.01 wt% / h.

[0075] Comparative Example 2

[0076] The preparation steps of the polytrimethylene terephthalate with low cyclic oligomer content of Comparative Example 2 are as follows:

[0077] Step (a), adding raw materials terephthalic acid and 1,3-propylene glycol into a polymerization reactor in a molar ratio of 1:2.2, and adding a catalyst tetrabutyl titanate in an amount of 300ppm of the total mass of terephthalic acid and 1,3-propylene glycol. The atmosphere in the polymerization reactor is replaced with nitrogen and then an esterification reaction is carried out. The temperature of the esterification reaction is 200°C, the pressure of the esterification reaction is 150KPaA, the stirring speed of the polymerization reactor is 50rpm, and the water output of the reaction system is recorded every 0.1h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid. The esterification reaction is terminated in a total of 4.5h.

[0078] Step (b), adding 50 ppm of aluminum trifluoromethanesulfonate to the esterification reaction liquid obtained in step (a), controlling the reaction system temperature to 220° C., the reaction system pressure to 200 PaA, and the stirring speed to 50 rpm, to carry out a pre-polycondensation reaction to obtain a pre-polycondensation reaction liquid (polytrimethylene terephthalate prepolymer), and the pre-polycondensation reaction lasts for 1.5 hours.

[0079] Step (c), adding 250ppm of (2,4,6-tri-tert-butylphenyl-2-butyl-2-ethyl)-1,3-propylene glycol phosphite to the pre-polycondensation reaction liquid obtained in step (b), controlling the temperature of the reaction system to 240°C, the vacuum degree of the reaction system to 20Pa, the stirring speed to 50rpm, and performing a post-polycondensation reaction. After reacting for 2.5h, stopping the reaction, discharging and granulating, and obtaining a poly(trimethylene terephthalate) product.

[0080] The polytrimethylene terephthalate product prepared in this embodiment was subjected to a PTT intrinsic viscosity test. The intrinsic viscosity of the polytrimethylene terephthalate product was 0.927 dL / g. The PTT intrinsic viscosity was tested according to the method of "FZ / T 51010-2014 Fiber-grade poly(trimethylene terephthalate) (PTT)". The solvent was phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40), and the Ubbelohde capillary viscometer was numbered 4-0.8.

[0081] The cyclic oligomer content of the poly(trimethylene terephthalate) prepared in this embodiment can be obtained by liquid chromatography after Soxhlet extraction. The poly(trimethylene terephthalate) is extracted using CH2Cl2 as a solvent, and the cyclic oligomer content in the extract is analyzed by liquid chromatography and its content in the polymer is calculated. The content of cyclic oligomers in the poly(trimethylene terephthalate) is 1.44wt% after liquid chromatography testing and calculation.

[0082] The generation rate of cyclic oligomers of the poly(trimethylene terephthalate) prepared in this embodiment during the melt processing was tested. The testing method was to remelt the prepared poly(trimethylene terephthalate) in a nitrogen atmosphere at a temperature of 260° C. and keep it for 0.5 h. Then, the cyclic oligomer content in the poly(trimethylene terephthalate) before and after remelting was analyzed, and the generation rate of the cyclic oligomers was calculated. After testing and calculation, the generation rate of cyclic oligomers in the poly(trimethylene terephthalate) was 0.82wt% / h.

[0083] Comparative Example 3

[0084] The preparation steps of the polytrimethylene terephthalate with low cyclic oligomer content of Comparative Example 3 are as follows:

[0085] Step (a), adding raw materials terephthalic acid and 1,3-propylene glycol into a polymerization reactor in a molar ratio of 1:1.7, adding a catalyst tetrabutyl titanate in an amount of 800 ppm of the total mass of terephthalic acid and 1,3-propylene glycol, replacing the atmosphere in the polymerization reactor with nitrogen and then performing an esterification reaction, the temperature of the esterification reaction is 220°C, the pressure of the esterification reaction is 350 KPaA, the stirring speed of the polymerization reactor is 100 rpm, discharging water generated by the reaction through a rectification device, recording the water output of the reaction system every 0.1 hour, and ending the esterification reaction when the water output of the reaction system reaches 90% of the theoretical water output, and the esterification reaction ends after a total of 3.5 hours.

[0086] After the step (b), the pressure is reduced to normal pressure after the esterification reaction is completed, and the prepolymer obtained in the step (a) is subjected to a precondensation reaction. The prepolymer reaction temperature is 240° C., the precondensation reaction pressure is 400 PaA, the stirring speed of the polymerization reactor is 100 rpm, and the precondensation reaction duration is 1 hour to obtain a precondensation reaction liquid.

[0087] Step (c), adding 500ppm of spiroethylene glycol di[2,2-methylenebis(4,6-di-tert-butylphenyl)]phosphite to the pre-polycondensation reaction liquid obtained in step (b), controlling the temperature of the reaction system to 260°C, the vacuum degree of the reaction system to 40Pa, the stirring speed to 100rpm, and carrying out a post-polycondensation reaction. After reacting for 1.5h, the reaction is stopped, and then the reactant is discharged from the bottom of the polymerization kettle and granulated to obtain a polytrimethylene terephthalate product.

[0088] The polytrimethylene terephthalate product prepared in the comparative example was subjected to a PTT intrinsic viscosity test. The intrinsic viscosity of the polytrimethylene terephthalate product was 0.845 dL / g. The PTT intrinsic viscosity was tested according to the method of "FZ / T 51010-2014 Fiber-grade poly(trimethylene terephthalate) (PTT)". Phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40) was used as the solvent, and the Ubbelohde capillary viscometer was numbered 4-0.8.

[0089] The cyclic oligomer content of the poly(trimethylene terephthalate) prepared in this comparative example can be obtained by liquid chromatography after Soxhlet extraction. The poly(trimethylene terephthalate) is extracted using CH2Cl2 as a solvent, and the cyclic oligomer content in the extract is analyzed by liquid chromatography and its content in the polymer is calculated. The content of cyclic oligomers in the poly(trimethylene terephthalate) is 2.66wt% after liquid chromatography testing and calculation.

[0090] The generation rate of cyclic oligomers of the poly(trimethylene terephthalate) prepared in the comparative example during the melt processing was tested. The testing method was as follows: the prepared poly(trimethylene terephthalate) was remelted in a nitrogen atmosphere at a temperature of 260°C and maintained for 0.5h. The cyclic oligomer content in the poly(trimethylene terephthalate) before and after remelting was analyzed, and the generation rate of the cyclic oligomers was calculated. After testing and calculation, the generation rate of the cyclic oligomers in the poly(trimethylene terephthalate) was found to be 1.44wt% / h.

[0091] Comparative Example 4

[0092] The preparation steps of the polytrimethylene terephthalate with low cyclic oligomer content of Comparative Example 4 are as follows:

[0093] Step (a), adding raw materials terephthalic acid and 1,3-propylene glycol into a polymerization reactor in a molar ratio of 1:2, adding a catalyst tetrabutyl titanate in an amount of 1000 ppm of the total mass of terephthalic acid and 1,3-propylene glycol, replacing the atmosphere in the polymerization reactor with nitrogen, and then carrying out an esterification reaction, the temperature of the esterification reaction is 230°C, the pressure of the esterification reaction is 250 KPaA, the stirring speed of the polymerization reactor is 150 rpm, discharging water generated by the reaction through a rectification device, recording the water output of the reaction system every 0.1 hour, and ending the esterification reaction when the water output of the reaction system reaches 90% of the theoretical water output, and the esterification reaction ends after a total of 2.5 hours.

[0094] Step (b), after the esterification reaction is completed, the pressure is reduced to normal pressure, and the prepolymer obtained in step (a) is subjected to a pre-polycondensation reaction. The pre-polycondensation reaction temperature is 250° C., the pre-polycondensation reaction pressure is 600 PaA, the stirring speed of the polymerization reactor is 100 rpm, and the pre-polycondensation reaction time is 1 h.

[0095] After the completion of the pre-polycondensation reaction in step (c), a post-polycondensation reaction is carried out. The temperature of the post-polycondensation reaction is 250° C., the vacuum degree of the post-polycondensation reaction is 60 Pa, and the stirring speed of the polymerization reactor is 100 rpm. After the post-polycondensation reaction for 2 hours, the reaction is stopped, and then the reactants are discharged from the bottom of the polymerization reactor and granulated to obtain a poly(trimethylene terephthalate) product.

[0096] The polytrimethylene terephthalate product prepared in this embodiment was subjected to a PTT intrinsic viscosity test. The intrinsic viscosity of the polytrimethylene terephthalate product was 0.749 dL / g. The PTT intrinsic viscosity was tested according to the method of "FZ / T 51010-2014 Fiber-grade poly(trimethylene terephthalate) (PTT)". The solvent was phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40), and the Ubbelohde capillary viscometer was numbered 4-0.8.

[0097] The cyclic oligomer content of the poly(trimethylene terephthalate) prepared in this embodiment can be obtained by liquid chromatography after Soxhlet extraction. The poly(trimethylene terephthalate) is extracted using CH2Cl2 as a solvent, and the cyclic oligomer content in the extract is analyzed by liquid chromatography and its content in the polymer is calculated. The content of cyclic oligomers in the poly(trimethylene terephthalate) is 3.11wt% after liquid chromatography testing and calculation.

[0098] The generation rate of cyclic oligomers of the poly(trimethylene terephthalate) prepared in this embodiment during the melt processing was tested. The testing method was to remelt the prepared poly(trimethylene terephthalate) in a nitrogen atmosphere at a temperature of 260° C. and maintain it for 0.5 h. Then, the cyclic oligomer content in the poly(trimethylene terephthalate) before and after remelting was analyzed, and the generation rate of the cyclic oligomers was calculated. After testing and calculation, the generation rate of the cyclic oligomers in the poly(trimethylene terephthalate) was 1.75 wt% / h.

[0099] Comparative Example 5

[0100] The preparation steps of the polyethylene terephthalate with low cyclic oligomer content of Example 5 are as follows:

[0101] Step (a), adding raw materials terephthalic acid and ethylene glycol in a molar ratio of 1:1.6 into a polymerization reactor, adding a catalyst tetra-n-butyl titanate in an amount of 1200ppm of the total mass of terephthalic acid and ethylene glycol, replacing the atmosphere in the polymerization reactor with nitrogen and then carrying out an esterification reaction, the esterification reaction temperature is 220°C, the esterification reaction pressure is 300KPaA, the stirring speed of the polymerization reactor is 180rpm, recording the water output of the reaction system every 0.1h, and when the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid, and the esterification reaction is terminated in a total time of 2.5h.

[0102] Step (b), adding 200 ppm of zinc trifluoromethanesulfonate to the esterification reaction liquid obtained in step (a), controlling the reaction system temperature to 260° C., the reaction system pressure to 1000 PaA, and the stirring speed to 200 rpm, and performing a pre-polycondensation reaction to obtain a pre-polycondensation reaction liquid (polyethylene terephthalate prepolymer), and the pre-polycondensation reaction duration is 0.8 h.

[0103] Step (c), adding 1000ppm of tris(2,4-di-tert-butylphenyl)phosphite to the pre-polycondensation reaction liquid obtained in step (b), controlling the temperature of the reaction system to 280°C, the vacuum degree of the reaction system to 100Pa, the stirring speed to 200rpm, and carrying out a post-polycondensation reaction. After reacting for 1h, stopping the reaction, discharging and granulating, and obtaining a polyethylene terephthalate product.

[0104] The PET intrinsic viscosity of the polyethylene terephthalate product prepared in this embodiment was tested. The intrinsic viscosity of the polyethylene terephthalate product was 0.915 dL / g. The PET intrinsic viscosity was tested according to the method of "GB / T 14190-2008 Test method for fiber-grade polyester chips (PET)". The solvent was phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40), and the Ubbelohde capillary viscometer was numbered 4-0.8.

[0105] The cyclic oligomer content of the polyethylene terephthalate prepared in this embodiment can be obtained by liquid chromatography after Soxhlet extraction. Use CH2Cl2 as a solvent to extract polyethylene terephthalate, analyze the cyclic oligomer content in the extract by liquid chromatography and calculate its content in the polymer. The content of cyclic oligomers in the polyethylene terephthalate is 1.62wt% after liquid chromatography testing and calculation.

[0106] The generation rate of cyclic oligomers of the polyethylene terephthalate prepared in this embodiment during the melt processing was tested. The testing method was to remelt the prepared polyethylene terephthalate in a nitrogen atmosphere at a temperature of 280° C. and maintain it for 0.5 h. Then, the cyclic oligomer content in the polyethylene terephthalate before and after remelting was analyzed, and the generation rate of the cyclic oligomers was calculated. After testing and calculation, the generation rate of the cyclic oligomers in the polyethylene terephthalate was 0.93wt% / h.

[0107] Comparative Example 6

[0108] The preparation steps of the polybutylene terephthalate with low cyclic oligomer content of Example 6 are as follows:

[0109] Step (a), adding raw materials terephthalic acid and 1,4-butanediol into a polymerization reactor in a molar ratio of 1:1.9, adding a catalyst tetrabutyl titanate in an amount of 900 ppm of the total mass of terephthalic acid and 1,4-butanediol, and performing an esterification reaction after the atmosphere in the polymerization reactor is replaced by nitrogen, the temperature of the esterification reaction is 210° C., the pressure of the esterification reaction is 250 KPaA, the stirring speed of the polymerization reactor is 120 rpm, and the water output of the reaction system is recorded every 0.1 h. When the water output of the reaction system reaches 90% of the theoretical water output, the esterification reaction is terminated to obtain an esterification reaction liquid, and the esterification reaction is terminated in a total time of 3.0 h.

[0110] Step (b), adding 120ppm of silicomolybdic acid to the esterification reaction liquid obtained in step (a), controlling the reaction system temperature to 240°C, the reaction system pressure to 400PaA, and the stirring speed to 120rpm, to carry out a pre-polycondensation reaction to obtain a pre-polycondensation reaction liquid (polybutylene terephthalate prepolymer), and the pre-polycondensation reaction lasts for 1.2h.

[0111] Step (c), adding 600ppm of spiroethylene glycol di[2,2-methylenebis(4,6-di-tert-butylphenyl)]phosphite to the pre-polycondensation reaction liquid obtained in step (b), controlling the temperature of the reaction system to 260°C, the vacuum degree of the reaction system to 50Pa, the stirring speed to 120rpm, and carrying out a post-polycondensation reaction. After reacting for 1.2h, stopping the reaction, discharging and granulating, and obtaining a polybutylene terephthalate product.

[0112] The polybutylene terephthalate product prepared in this embodiment was tested for its PBT intrinsic viscosity. The intrinsic viscosity of the polybutylene terephthalate product was 0.884 dL / g. The PBT intrinsic viscosity was tested according to the method of "HG / T 5510-2019 Plastic Polybutylene Terephthalate (PBT) Resin". The solvent was phenol / 1,1,2,2-tetrachloroethane (mass ratio 60:40), and the Ubbelohde capillary viscometer was numbered 4-0.8.

[0113] The cyclic oligomer content of the polybutylene terephthalate prepared in this embodiment can be obtained by liquid chromatography after Soxhlet extraction. Use CH2Cl2 as a solvent to extract polybutylene terephthalate, analyze the cyclic oligomer content in the extract by liquid chromatography and calculate its content in the polymer. The content of cyclic oligomers in the polybutylene terephthalate obtained by liquid chromatography and calculation is 1.91wt%.

[0114] The generation rate of cyclic oligomers of the polybutylene terephthalate prepared in this embodiment during the melt processing was tested. The testing method was to remelt the prepared polybutylene terephthalate in a nitrogen atmosphere at a temperature of 260° C. and maintain it for 0.5 h. Then, the cyclic oligomer content in the polybutylene terephthalate before and after remelting was analyzed, and the generation rate of the cyclic oligomers was calculated. After testing and calculation, the generation rate of the cyclic oligomers in the polybutylene terephthalate was 1.05wt% / h.

[0115] Table 1 Comparison table of embodiments and comparative examples

[0116]

[0117]

[0118] As can be seen from Table 1, in the polymerization reaction process of preparing terephthalic acid-based polyesters in Examples 1 to 6, a certain amount of trifluoromethanesulfonate catalyst and heteropolyacid catalyst were added, and while obtaining high intrinsic viscosity terephthalic acid-based polyester ester products, the intrinsic viscosity of the terephthalic acid-based polyesters in Examples 1 to 6 was 0.996-1.073 dL / g, the amount of by-product cyclic oligomers generated was significantly reduced, the content of cyclic oligomers in Examples 1 to 6 was 0.29-0.35wt%, and it was difficult to generate cyclic oligomers during the remelting process, which effectively improved the product quality and processing stability. Since organic phthalates are common polyester catalysts, they have the advantages of high catalytic activity and good ecological safety. However, it cannot effectively solve the problem that the terminal hydroxyl groups of polyester will bite back in the melt to generate cyclic oligomer by-products. The combination of trifluoromethanesulfonate and heteropolyacid catalysts can effectively open the ring structure of the cyclic oligomers generated in the polyester melt and re-add it to the polycondensation process, thereby reducing the content of by-products in the product. Since the trifluoromethanesulfonate and heteropolyacid structures are stable and evenly dispersed in the product, even in the re-melting process, trifluoromethanesulfonate and heteropolyacid can still play a role, which can effectively inhibit the regeneration of cyclic oligomers, thereby further avoiding the occurrence of "frosting" and "white fog" during the processing process, and can effectively improve its processing stability and product quality.

[0119] In Comparative Example 1, only a heteropolyacid catalyst is added during the pre-polycondensation reaction, but no trifluoromethanesulfonate catalyst is added. The cyclic oligomer content of the poly(trimethylene terephthalate) in Comparative Example 1 is higher than that in Example 1. The content of cyclic oligomers of the poly(trimethylene terephthalate) prepared in Comparative Example 1 is 1.83wt%. Compared with Example 1, the content of cyclic oligomers of the poly(trimethylene terephthalate) prepared in Example 1 is 0.31wt%. Therefore, when only a heteropolyacid catalyst is added in Comparative Example 1, but no trifluoromethanesulfonic acid catalyst is added, it is not easy to open the cyclic oligomer ring structure generated in the PTT melt again during the preparation process, and it is not re-added to the polycondensation process. Therefore, the content of by-product cyclic oligomers in Comparative Example 1 is higher than that in Example 1.

[0120] In Comparative Example 2, only trifluoromethanesulfonic acid catalysts were added during the pre-polycondensation reaction, and no heteropolyacid catalysts were added. Compared with Example 2, the intrinsic viscosity of the poly(trimethylene terephthalate) in Comparative Example 2 was lower than that in Example 1, while the content of cyclic oligomers in Comparative Example 2 was higher than that in Example 2, and the generation rate of cyclic oligomers in Comparative Example 2 was higher than that in Example 2. Therefore, when only trifluoromethanesulfonic acid catalysts were added in Comparative Example 2, it was also not easy to open the cyclic oligomer ring structure generated in the PTT melt again during the preparation process, and it was not re-added to the polycondensation process. Therefore, the content of by-product cyclic oligomers in Comparative Example 2 was higher than that in Example 2.

[0121] Trifluoromethanesulfonic acid catalyst and heteropolyacid catalyst were not added in Comparative Example 3, and its intrinsic viscosity was lower than the viscosity with the addition of trifluoromethanesulfonic acid catalyst and heteropolyacid catalyst, and the content of the cyclic oligomer without the addition of trifluoromethanesulfonic acid catalyst and heteropolyacid catalyst was much higher than that with the addition of trifluoromethanesulfonic acid catalyst and heteropolyacid catalyst, and similarly, the generation rate of the cyclic oligomer without the addition of trifluoromethanesulfonic acid catalyst and heteropolyacid catalyst was also much higher than that with the addition of trifluoromethanesulfonic acid catalyst and heteropolyacid catalyst.

[0122] Comparative Examples 5 and 6 illustrate that this method is also applicable to the preparation of PET and PBT with low cyclic oligomer content.

[0123] It can be seen that the present application can effectively reopen the cyclic oligomer ring structure generated in the terephthalic acid-based polyester melt by adding trifluoromethanesulfonate and heteropolyacid catalysts, and re-add it to the polycondensation process, thereby reducing the content of by-products in the product. Even in the melt processing process, it is difficult to produce by-product cyclic oligomers, which greatly reduces the content of cyclic oligomers. In addition, the catalysts and additives used in the present application are not only non-toxic and inexpensive, but are also conventional commercial products, which are easy to purchase in the market and have high industrial application value. In addition, the preparation method does not change the existing process flow, and can use the existing polyester device for direct production, so no additional economic investment is required.

[0124] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing terephthalate-based polyester, characterized in that: The method comprises the following preparation steps: Step (a), mixing terephthalic acid, diol and organic titanium catalyst in a certain proportion, and carrying out esterification reaction at a certain temperature, pressure and stirring speed to obtain an esterification reaction liquid; Step (b), adding a certain amount of trifluoromethanesulfonate catalyst and heteropolyacid catalyst to the esterification reaction liquid obtained in step (a), and performing a pre-polycondensation reaction at a certain temperature, pressure and stirring speed to obtain a pre-polycondensation reaction liquid; Step (c), adding a certain amount of phosphite antioxidant to the pre-polycondensation reaction liquid obtained in step (b), and performing post-polycondensation reaction at a certain temperature, pressure and stirring speed to obtain a product terephthalic acid-based polyester.

2. The preparation method according to claim 1, characterized in that: In the step (a), the organic titanium catalyst includes one or more of ethylene glycol titanium, propylene glycol titanium, butanediol titanium, tetraethyl titanate, tetraisopropyl titanate, tetra-n-propyl titanate, and tetra-n-butyl titanate; the diol includes one of ethylene glycol, 1,3-propylene glycol, and 1,4-butanediol.

3. The preparation method according to claim 2, characterized in that: In the step (a), the molar ratio of the added amount of terephthalic acid to the diol is 1:1.4-2.2, and the added amount of the organic titanium catalyst is 300-1500 ppm of the total mass of the terephthalic acid and the diol.

4. The preparation method according to claim 3, characterized in that: In the step (a), the esterification reaction temperature is 200-240° C.; the esterification reaction pressure is 150-400 KPaA; the esterification reaction time is 2-4.5 h; and the stirring speed is 50-200 rpm.

5. The preparation method according to claim 1, characterized in that: In the step (b), the trifluoromethanesulfonate catalyst includes one or more of zinc trifluoromethanesulfonate, scandium trifluoromethanesulfonate, indium trifluoromethanesulfonate, aluminum trifluoromethanesulfonate, cerium trifluoromethanesulfonate, and copper trifluoromethanesulfonate; the amount of the trifluoromethanesulfonate catalyst added is 50 to 250 ppm of the total mass of the terephthalic acid and the diol.

6. The preparation method according to claim 5, characterized in that: In the step (b), the heteropoly acid catalyst includes one or more of phosphotungstic acid, silicotungstic acid, phosphomolybdic acid, and silicomolybdic acid, and the added amount of the heteropoly acid catalyst is 50 to 250 ppm of the total mass of the terephthalic acid and the diol.

7. The preparation method according to claim 6, characterized in that: In the step (b), the pre-polycondensation temperature is 220-260° C.; the pre-polycondensation pressure is 200-1000 PaA; the pre-polycondensation reaction time is 0.5-1.5 h; and the stirring speed is 50-200 rpm.

8. The preparation method according to claim 1, characterized in that: In the step (c), the phosphite antioxidant includes one or more of tris(2,4-di-tert-butylphenyl)phosphite, bis[2-methyl-4,6-bis(1,1'-dimethylethyl)phenol]ethyl phosphate, tetrakis(2,4-di-tert-butyloctaalkoxy-4,4-biphenylyl)phosphate, pentaerythritol bis(2,4-tert-butylphenyl)diphosphite, (2,4,6-tri-tert-butylphenyl-2-butyl-2-ethyl)-1,3-propylene glycol phosphite, di(2,4-di-p-isopropylphenyl)pentaerythritol bisphosphite, 2,2'-ethylenebis(4,6-di-tert-butylphenyl)fluorophosphite, tetrakis(2,4-di-tert-butylphenyl-4,4-biphenylyl)bisphosphate, and spiroethylene glycol di[2,2'-methylenebis(4,6-di-tert-butylphenyl)]phosphite.

9. The preparation method according to claim 8, characterized in that: In the step (c), the amount of the phosphite antioxidant added is 250 to 1000 ppm of the pre-polycondensation reaction liquid; the temperature of the post-polycondensation is 240 to 280° C.; the vacuum degree of the post-polycondensation is 20 to 100 Pa; and the time of the post-polycondensation is 1 to 2.5 hours.

10. The preparation method according to claim 1, characterized in that: The cyclic oligomer content of the prepared terephthalic acid-based polyester is less than 0.35wt%; the generation rate of the cyclic oligomer of the prepared terephthalic acid-based polyester is less than 0.16wt% / h; the intrinsic viscosity of the prepared terephthalic acid-based polyester is 0.996-1.073dL / g.