Polyimide resin and application thereof
By introducing polyimide resins with amide structures and nitro groups, the problems of deformation and insufficient absorption rate of transfer adhesive under high-temperature processes were solved, achieving high temperature resistance and high transfer yield, reducing chip damage and residual adhesive, and improving chip quality.
Patent Information
- Application Number
- CN202411134569.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
In existing mass transfer processes, high-temperature processes cause deformation of the transfer adhesive, affecting chip positioning. Furthermore, the absorption rate of the transfer adhesive is insufficient at high temperatures, resulting in residual adhesive and carbon particles, which affect transfer yield and chip quality.
Using polyimide resin, by introducing amide structure and nitro group, the intermolecular forces are enhanced, the glass transition temperature is increased, the ultraviolet absorption capacity is increased, the 355nm wavelength process is met, the damage of laser energy to the chip is reduced and the residue is avoided.
It improves the temperature resistance and transfer yield of the transfer adhesive, reduces the damage of laser energy to the chip, ensures no adhesive residue, and improves chip quality.
Smart Images

Figure CN119019687A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mass transfer and relates to a polyimide resin and an application thereof. Background Art
[0002] In mass transfer, the surface of the Sapphire substrate (including LED) is attached with a transfer release tape (including transfer glue and carrier 1), and the laser is transmitted through the Sapphire to irradiate the LED; after laser irradiation, the LED is separated from the Sapphire, the entire Sapphire is peeled off, and the LED is stuck to the fixed position of the transfer tape; after the transfer is aligned, the laser is transmitted through the carrier 1 to irradiate the transfer release glue, which absorbs light energy and sublimates and vaporizes, and the LED falls on the specified position of the receiving tape (including receiving glue and carrier 2); the receiving tape is aligned with the TFT backplane, and the laser is transmitted through the carrier 2 to irradiate the receiving glue, which absorbs light energy and sublimates and vaporizes, and the LED falls on the specified position of the backplane (sub-pixel position), and then the subsequent process is carried out.
[0003] However, in the current mass transfer process, the process after the LED is separated from Sapphire involves high temperature. The existing transfer glue has too low Tg, and the high temperature process causes it to deform due to heat, resulting in changes in the chip position. In addition, the existing transfer glue has insufficient absorption rate in a specific wavelength range, resulting in incomplete ablation and gasification of the transfer glue. As a result, there will be residual glue or carbon particles after laser ablation of the transfer glue, which are located near the chip pins, affecting the transfer yield, causing great damage to the chip and affecting the chip quality.
[0004] Therefore, in the art, it is desired to develop materials that can avoid the above defects caused by high temperature processes to improve chip quality. Summary of the invention
[0005] In view of the deficiencies in the prior art, an object of the present invention is to provide a polyimide resin and application thereof.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] One of the purposes of the present invention is to provide a polyimide resin having a structure shown in Formula I:
[0008]
[0009] Where R1 is Y1 is an ether or thioether group, Y2 is absent or selected from a C1-C5 straight or branched alkyl group, a carbonyl group, a C1-C5 alkyl-carbonyl group, an ether group or a thioether group;
[0010] R2 is selected from X is selected from an ether group, a thioether group, a C1-C10 straight or branched alkyl group, a carbonyl group or a C1-C5 straight or branched alkyl-carbonyl group, and R3 and R4 are independently selected from a nitro group or R7 is selected from alkenyl or alkynyl; R5 and R6 are independently selected from halogen, C1-C5 alkyl, C3-C6 cycloalkyl, C1-C5 alkoxy, C6-C12 aryl or C3-C12 heteroaryl;
[0011] n is selected from an integer of 100-500, n1, n2, n3 and n4 are independently selected from integers of 0-4, n1 and n3 are not 0 at the same time, and n1+n3≤4, n2+n4≤4.
[0012] In the present invention, due to the introduction of amide structure or nitro group in the polyimide resin, the intermolecular force is increased through a large number of hydrogen bonds, the glass transition temperature Tg of the polymer material is increased, and the adhesion between the material and the substrate is enhanced by introducing ether bond through R1, so as to avoid the influence of decreased adhesion due to the increase of Tg. In addition, the introduction of amide bond and the introduction of nitro group and ether bond in the polyimide resin of the present invention causes red shift in the ultraviolet absorption of the material, so that it has stronger absorption above 300nm, which can meet the process of 355nm wavelength.
[0013] When the polyimide resin of the present invention is used for transfer glue, it can ensure that the transfer glue has better temperature resistance, has a wide range of options for subsequent processes, and has a high transfer yield; it can correspond to a 355nm laser wavelength ablation process, has low laser energy, less damage to the chip, and has no residual glue.
[0014] A second object of the present invention is to provide a transfer adhesive, wherein the transfer adhesive comprises the polyimide resin as described in the first object.
[0015] The third object of the present invention is to provide a receiving adhesive, wherein the receiving adhesive comprises the polyimide resin as described in the first object.
[0016] A fourth object of the present invention is to provide the use of the polyimide resin as described in the first object, the transfer adhesive as described in the second object, or the receiving adhesive as described in the third object in mass transfer.
[0017] A fifth object of the present invention is to provide a mass transfer method, which comprises using the polyimide resin as described in one of the objects as a transfer adhesive.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The polyimide resin of the present invention has a higher glass transition temperature and stronger absorption above 300nm, and can meet the process of 355nm wavelength. When the polyimide resin of the present invention is used for transfer glue, it can ensure that the transfer glue has better temperature resistance, has a large range of options for subsequent processes, and has a high transfer yield; it can correspond to the 355nm laser wavelength ablation process, has low laser energy, less damage to the chip, and no residual glue. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a schematic diagram of the mass transfer process flow, where 1 is the Sapphire substrate, 2 is the transfer glue, 3 is the first carrier, 4 is the receiving glue, 5 is the second carrier, and 6 is the backplane. DETAILED DESCRIPTION
[0021] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0022] One of the purposes of the present invention is to provide a polyimide resin having a structure shown in Formula I:
[0023]
[0024] Where R1 is Y1 is an ether or thioether group, Y2 is absent or selected from a C1-C5 straight or branched alkyl group, a carbonyl group, a C1-C5 alkyl-carbonyl group, an ether group or a thioether group;
[0025] R2 is selected from X is selected from an ether group, a thioether group, a C1-C10 straight or branched alkyl group, a carbonyl group or a C1-C5 straight or branched alkyl-carbonyl group, and R3 and R4 are independently selected from a nitro group or R7 is selected from alkenyl or alkynyl; R5 and R6 are independently selected from halogen, C1-C5 alkyl, C3-C6 cycloalkyl, C1-C5 alkoxy, C6-C12 aryl or C3-C12 heteroaryl;
[0026] n is selected from an integer of 100-500, n1, n2, n3 and n4 are independently selected from integers of 0-4, n1 and n3 are not 0 at the same time, and n1+n3≤4, n2+n4≤4.
[0027] In the present invention, due to the introduction of amide structure or nitro group in the polyimide resin, the intermolecular force is increased through a large number of hydrogen bonds, the glass transition temperature Tg of the polymer material is increased, and the adhesion between the material and the substrate is enhanced by introducing an ether bond through R1, thereby avoiding the influence of decreased adhesion due to the increase in Tg. In addition, the introduction of amide bonds with unsaturated groups (i.e., alkenyl or alkynyl) and the introduction of nitro and ether bonds in the polyimide resin of the present invention causes a red shift in the ultraviolet absorption of the material, so that it has stronger absorption above 300nm, which can meet the process of 355nm wavelength.
[0028] When the polyimide resin of the present invention is used for transfer glue, it can ensure that the transfer glue has better temperature resistance, has a wide range of options for subsequent processes, and has a high transfer yield; it can correspond to a 355nm laser wavelength ablation process, has low laser energy, less damage to the chip, and has no residual glue.
[0029] In the present invention, the C1-C5 may be C1, C2, C3, C4 or C5; the C1-C10 may be C1, C2, C3, C4, C5, C6, C7, C8, C9 or C10; the C3-C6 may be C3, C4, C5 or C6; the C6-C12 may be C6, C7, C8, C9, C10, C11 or C12; the C3-C12 may be C3, C4, C5, C6, C7, C8, C9, C10, C11 or C12.
[0030] In the present invention, n is selected from an integer of 100-500, for example, 100, 103, 105, 108, 110, 120, 130, 240, 150, 170, 190, 200, 220, 240, 250, 280, 300, 320, 350, 380, 400, 420, 450, 480 or 500, etc. In the present invention, n represents the number of repeating units in Formula I.
[0031] In the present invention, n1, n2, n3 and n4 are independently selected from integers of 0-4, such as 0, 1, 2, 3 or 4.
[0032] In the present invention, n1 and n3 are not 0 at the same time. In the present invention, by introducing an amide structure or a nitro group into the structure shown in Formula I, more hydrogen bonds can be present in the polyimide resin structure, thereby increasing the intermolecular force and improving the glass transition temperature of the polymer material.
[0033] In the present invention, n1+n3≤4, for example, n1+n3 can be 0, 1, 2, 3, 4, and n2+n4≤4, for example, n2+n4 can be 0, 1, 2, 3, 4.
[0034] In the present invention, R1 is Y1 is an ether or thioether group, and Y2 is absent or selected from C1-C5 straight or branched alkyl, carbonyl, C1-C5 alkyl-carbonyl, ether group or thioether group. In the present invention, Y1 in R1 is an ether or thioether group, and Y2 may be absent or any one of the groups described above. When Y2 is absent, it means that there is no connecting bond at Y2, that is, R1 is
[0035]
[0036] In some embodiments, the ether group is selected from O-, wherein m and p are independently integers of 1-5, such as 1, 2, 3, 4 or 5.
[0037] In some embodiments, the thioether group is selected from -S-, wherein m1 and p1 are independently integers of 1-5, such as 1, 2, 3, 4 or 5.
[0038] In some embodiments, R1 is Wherein Y3 is selected from O or S, Y4 is selected from C1-C5 straight chain or branched alkyl, carbonyl, C1-C5 alkyl-carbonyl, ether group or thioether group, and m2 is selected from an integer of 1-5.
[0039] In some embodiments, Y4 is selected from -O-, -S-, carbonyl,
[0040] In some embodiments, R1 is
[0041] In the present invention, n1 and n3 are not 0 at the same time, so that R2 includes at least one R3 or R4 group, so that its structure contains nitro or Structure, that is, a nitro group or an amide structure with an α, β-unsaturated group is introduced into the polyimide resin structure, which causes the ultraviolet absorption of the material to red-shift, making it have stronger absorption above 300nm and able to meet the 355nm wavelength process.
[0042] In some embodiments, X is selected from -CH2-, -S-, m, p, m1 and p1 are independently an integer of 1-5, such as 1, 2, 3, 4 or 5.
[0043] In some embodiments, the alkenyl group is selected from C2-C8 alkenyl groups, such as C2, C3, C4, C5, C6, C7 or C8 alkenyl groups, and specific examples may be Etc., the wavy lines represent the attachment sites of the groups.
[0044] In some embodiments, the alkynyl group is selected from C2-C8 alkynyl groups, such as C2, C3, C4, C5, C6, C7 or C8 alkynyl groups, and specific examples may be Etc., the wavy lines represent the attachment sites of the groups.
[0045] In some embodiments, the R7 is selected from The wavy line represents the attachment site of the group.
[0046] In some embodiments, R3 and R4 are independently selected from nitro,
[0047] In some embodiments, R3 and R4 are selected from the same group. When R3 and R4 are selected from the same group, the molecular structure is more symmetrical, has a greater intermolecular force, and can further increase the Tg of the final material.
[0048] In some embodiments, R5 and R6 are independently selected from hydrogen, F, Cl, Br, methyl, ethyl, isopropyl, pentyl, cyclopropyl, cyclohexyl, methoxy, ethoxy, phenyl, biphenyl, naphthyl, pyridyl, furanyl, triazinyl, benzofuranyl or dibenzofuranyl.
[0049] In the present invention, the structure of R2 There may be a case where it contains only R3 substituent, or a case where it contains only R4 substituent, or a case where it contains both R3 and R4 substituents but does not contain R5 and R6 substituents, or a case where it contains R3 and R4 and at least one of R5 and R6.
[0050] In some preferred embodiments, R2 is selected from R3, R4, X, n1 and n2 are as defined above.
[0051] In some preferred embodiments, R2 is selected from R3, R4, and X are as defined above.
[0052] In some preferred embodiments, R2 is selected from X is defined as above.
[0053] In some embodiments, the polyimide resin has a structure of any one of the following formulas II to VI:
[0054]
[0055] wherein n and X are as defined above.
[0056] In some embodiments, the polyimide resin is any one of the following compounds:
[0057]
[0058]
[0059]
[0060]
[0061] wherein n is selected from an integer of 100-500.
[0062] A second object of the present invention is to provide a transfer adhesive, wherein the transfer adhesive comprises the polyimide resin as described in the first object.
[0063] When the polyimide resin of the present invention is used for transfer glue, it can ensure that the transfer glue has better temperature resistance, has a wide range of options for subsequent processes, and has a high transfer yield; it can correspond to a 355nm laser wavelength ablation process, has low laser energy, less damage to the chip, and has no residual glue.
[0064] The third object of the present invention is to provide a receiving adhesive, wherein the receiving adhesive comprises the polyimide resin as described in the first object.
[0065] A fourth object of the present invention is to provide the use of the polyimide resin as described in the first object, the transfer adhesive as described in the second object, or the receiving adhesive as described in the third object in mass transfer.
[0066] A fifth object of the present invention is to provide a mass transfer method, which comprises using the polyimide resin as described in one of the objects as a transfer adhesive.
[0067] The mass transfer method may include the following steps:
[0068] like Figure 1As shown, a transfer release tape (including transfer glue 2 and a first carrier 3) is attached to the surface of a Sapphire substrate 1 (including an LED), and a laser is transmitted through the Sapphire to irradiate the LED; after laser irradiation, the LED is separated from the Sapphire, the Sapphire is peeled off as a whole, and the LED is adhered to a fixed position of the transfer release tape; after transfer alignment, the laser is transmitted through the first carrier 3 to irradiate the transfer release glue, which absorbs light energy and sublimates and vaporizes, and the LED falls on a specified position of a receiving tape (including a receiving glue 4 and a second carrier 5); the receiving tape is aligned with a TFT backplane 6, and the laser is transmitted through the second carrier 5 to irradiate the receiving glue, which absorbs light energy and sublimates and vaporizes, and the LED falls on a specified position of the backplane (a sub-pixel position), and then subsequent processes are performed; wherein the polyimide resin described in one of the purposes of the present invention is used as the transfer glue.
[0069] In the present invention, the first carrier and the second carrier can be selected from common transparent substrates such as PET.
[0070] In the present invention, when the polyimide resin is used as the transfer adhesive, the receiving adhesive may be selected from one or a combination of at least two of silicone resin, polyimide resin, acrylic resin or polyurethane resin.
[0071] Several examples of preparing the polyimide resin of the present invention are listed below:
[0072] Example 1
[0073] This embodiment provides a polyimide having the following structure:
[0074]
[0075] Here, X is an oxygen atom.
[0076] The preparation method comprises the following steps:
[0077] (1) Preparation of diamine monomer
[0078] Under nitrogen atmosphere and room temperature, 200 mL of tetrahydrofuran (THF) solvent, triethylamine and 3,3,4,4-tetraaminodiphenyl ether in a molar ratio of 1:1 were added to a three-necked flask. In an ice-water bath, 1.1 equivalents of 2-butenoyl chloride were slowly added dropwise. The reaction was stirred for 2 h, and the precipitate was removed by filtration. The reaction solution was separated by column chromatography, concentrated, and recrystallized to obtain product A.
[0079] (2) Preparation of polyamic acid
[0080] In a three-necked flask, add anhydride B at a 1:1 molar ratio. and product A, and reacted in dimethylacetamide solvent at room temperature with stirring for 9 hours to obtain a polyamic acid precursor, wherein n is 100-200.
[0081]
[0082] (3) Preparation of polyimide
[0083] Dissolve polyamic acid in dimethylacetamide to obtain a precursor solution with a mass percentage concentration of 45%, apply it to form a film, heat it to 180°C to dry the solvent, keep it at 200°C for 3h, keep it at 260°C for 5h, keep it at 230°C for 3h, slowly return to room temperature to obtain a polyimide product, and its glass transition temperature (Tg) is 290°C and the ultraviolet absorption cutoff wavelength is 320nm. The glass transition temperature (Tg) is obtained by TA DMA 850 test, and the ultraviolet absorption test uses Aglient 8453.
[0084] Example 2
[0085] This embodiment provides a polyimide having the following structure:
[0086]
[0087] Here, X is a sulfur atom.
[0088] The synthesis method is the same as that in Example 1, except that the raw material 3,3,4,4-tetraaminodiphenyl ether is replaced by 3,3,4,4-tetraaminodiphenyl sulfide.
[0089] The obtained polyimide product has a glass transition temperature of 280° C. and an ultraviolet absorption cutoff wavelength of 330 nm.
[0090] Example 3
[0091] This embodiment provides a polyimide having the following structure:
[0092]
[0093] Here, X is an oxygen atom or a sulfur atom.
[0094] The synthesis method is the same as that in Example 1, and the raw materials 3,3,4,4-tetraaminodiphenyl ether and 3,3,4,4-tetraaminodiphenyl sulfide are used in a molar ratio of 9:1.
[0095] The polyimide product was obtained, and its Tg was 280° C. and its ultraviolet absorption cutoff wavelength was 320 nm.
[0096] Example 4
[0097] This embodiment provides a polyimide having the following structure:
[0098]
[0099] Here, X is an oxygen atom or a sulfur atom.
[0100] The synthesis method is the same as that of Example 1, wherein the diamine is 4,4'-diamino-3,3'-dinitrodiphenyl ether or 4,4'-diamino-3,3'-dinitrodiphenyl sulfide, and the molar ratio is 8:3.
[0101] The obtained polyimide product has a Tg of 310° C. and an ultraviolet absorption cutoff wavelength of 340 nm.
[0102] Comparative Example 1
[0103] The polyamic acid prepared in Example 1 of CN104804434B was used as a comparative compound, and its structure is as follows:
[0104]
[0105] Comparative Example 2
[0106] This comparative example provides a polyimide having the following structure:
[0107]
[0108] The synthesis method of this comparative example is the same as that of Example 1, wherein the dianhydride is 4,4'-biphenyl ether dianhydride, and the diamine is 4,4'-diaminodiphenyl ether.
[0109] The obtained polyimide product has a Tg of 260° C. and an ultraviolet absorption cutoff wavelength of 240 nm.
[0110] Application Examples 1-4 and Comparative Application Examples 1-2
[0111] The polyimide prepared in Examples 1-4 and Comparative Examples 1-2 is used as a transfer adhesive to perform mass transfer, which includes the following steps (the process steps are as follows Figure 1 shown):
[0112] (1) A transfer release tape (transfer adhesive 2 + first carrier 3) is attached to the surface of a Sapphire substrate 1 (containing a light-emitting element LD, such as an LED), wherein the transfer adhesive 2 is the polyimide prepared in an embodiment or a comparative example of the present invention, and the first carrier 3 is PET. Laser is transmitted through the Sapphire to irradiate the LED;
[0113] (2) After laser irradiation, the LED is separated from the Sapphire, and the Sapphire is peeled off as a whole, and the LED is stuck to the fixed position of the transfer release tape;
[0114] (3) After the transfer and alignment, the laser is irradiated on the transfer release adhesive through the first carrier 3. After absorbing the light energy, it sublimates and vaporizes, and the LED falls on the specified position of the receiving tape (receiving adhesive 4 + second carrier 5); the receiving adhesive 4 is made of silicone resin, and the second carrier 5 is PET.
[0115] (4) The receiving tape is aligned with the TFT backplane 6, and the laser is irradiated on the receiving tape through the second carrier 5. After absorbing the light energy, it sublimates and vaporizes, and the LED falls on the specified position of the backplane (sub-pixel position), completing the mass transfer, and then proceeding to the subsequent process.
[0116] The transfer yield of mass transfer in the corresponding use case, including transfer accuracy and residual glue rate, is evaluated. The specific method is as follows:
[0117] (1) Transfer yield: The percentage of LED chips that can light up after transfer is counted out of every 100,000 LED chips.
[0118] (2) Glue residue rate: Count the number of LED chips with glue residue on them out of every 100,000 LED chips transferred.
[0119] The evaluation results are shown in Table 1.
[0120] Table 1
[0121] Transfer yield Residual glue rate Application Example 1 99.5% 0.85% Application Example 2 99.94% 0.082% Application Example 3 99.996% 0.004% Application Example 4 99.995% 0.005% Comparative Example 1 0 (no stickiness, cannot be transferred) / Comparative Example 2 80% 1.5%
[0122] It can be seen that the polyimide resin of the present invention as transfer adhesive can achieve a transfer yield of more than 99.95% and reduce the residual adhesive rate to less than 0.85%.
[0123] The applicant declares that the present invention illustrates the polyimide resin and its application through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A polyimide resin, characterized in that: The polyimide resin has a structure shown in Formula I: Where R1 is Y1 is an ether or thioether group, Y2 is absent or selected from a C1-C5 straight or branched alkyl group, a carbonyl group, a C1-C5 alkyl-carbonyl group, an ether group or a thioether group; R2 is selected from X is selected from an ether group, a thioether group, a C1-C10 straight or branched alkyl group, a carbonyl group or a C1-C5 straight or branched alkyl-carbonyl group, and R3 and R4 are independently selected from a nitro group or R7 is selected from alkenyl or alkynyl; R5 and R6 are independently selected from hydrogen, halogen, C1-C5 alkyl, C3-C6 cycloalkyl, C1-C5 alkoxy, C6-C12 aryl or C3-C12 heteroaryl; n is selected from an integer of 100-500, n1, n2, n3 and n4 are independently selected from integers of 0-4, n1 and n3 are not 0 at the same time, n1+n3≤4, n2+n4≤4.
2. The polyimide resin according to claim 1, characterized in that The ether group is selected from O-, wherein m and p are independently integers of 1-5.
3. The polyimide resin according to claim 1, characterized in that The thioether group is selected from -S-, wherein m1 and p1 are independently integers of 1-5.
4. The polyimide resin according to claim 1, characterized in that R1 is Wherein Y3 is selected from O or S, Y4 is selected from C1-C5 straight chain or branched alkyl, carbonyl, C1-C5 alkyl-carbonyl, ether group or thioether group, and m2 is selected from an integer of 1-5.
5. The polyimide resin according to claim 4, characterized in that Y4 is selected from -O-, -S-, carbonyl, -CH2- or 6. The polyimide resin according to claim 1 or 4, characterized in that: R1 is 7. The polyimide resin according to claim 1, characterized in that X is selected from -CH2-, O-, -S-, m, p, m1 and p1 are independently integers of 1-5.
8. The polyimide resin according to claim 1, characterized in that The alkenyl group is selected from C2-C8 alkenyl groups.
9. The polyimide resin according to claim 1, characterized in that The alkynyl group is selected from C2-C8 alkynyl groups.
10. The polyimide resin according to claim 1, characterized in that The R7 is selected from The wavy line represents the attachment site of the group.
11. The polyimide resin according to claim 1, characterized in that R3 and R4 are independently selected from nitro, 12. The polyimide resin according to claim 1 or 11, characterized in that: R3 and R4 are selected from the same group.
13. The polyimide resin according to claim 1, characterized in that R5 and R6 are independently selected from hydrogen, F, Cl, Br, methyl, ethyl, isopropyl, pentyl, cyclopropyl, cyclohexyl, methoxy, ethoxy, phenyl, biphenyl, naphthyl, pyridyl, furanyl, triazinyl, benzofuranyl or dibenzofuranyl.
14. The polyimide resin according to claim 1, characterized in that R2 is selected from R3, R4, X, n1 and n2 are as defined in claim 1.
15. The polyimide resin according to claim 1, characterized in that R2 is selected from R3, R4, and X are as defined in claim 1.
16. The polyimide resin according to claim 15, characterized in that R2 is selected from X is as defined in claim 1.
17. The polyimide resin according to claim 1, characterized in that The polyimide resin has any one of the following structures: wherein n and X are as defined in claim 1.
18. The polyimide resin according to claim 1, characterized in that The polyimide resin is any one of the following compounds: wherein n is selected from an integer of 100-500.
19. A transfer adhesive, characterized in that: The transfer adhesive comprises the polyimide resin according to any one of claims 1 to 18.
20. A bonding adhesive, characterized in that: The receiving adhesive comprises the polyimide resin as described in any one of claims 1-18.
21. Use of the polyimide resin according to any one of claims 1 to 18, the transfer adhesive according to claim 19, or the receiving adhesive according to claim 20 in mass transfer.
22. A method for mass transfer, characterized in that: The mass transfer method comprises using the polyimide resin as described in any one of claims 1 to 18 as a transfer adhesive.
Citation Information
Patent Citations
A polyimide film, a composition and method for preparing the polyimide film, and a flexible circuit board and its preparation method.
CN104804434B
Cited By
Temporary bonding glue and application thereof
CN121343546A
Temporary bonding adhesive and its use