Photovoltaic cable and preparation process thereof

By using mixtures of materials such as ethylene-octene copolymers and electron beam crosslinking technology in photovoltaic cables, combining aluminum hydroxide and magnesium borate whisker composites and modified aramid fiber nanosilica fillers, traditional photovoltaics are solved The problem of insufficient weather resistance and wear resistance of cables significantly improves the flame retardant and mechanical properties of cables and extends the service life.

CN119019779AInactive Publication Date: 2024-11-26JIANGSU DONGXU CABLE CO LTD

Patent Information

Application Number
CN202411341661.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional photovoltaic cables are inadequate weather resistance, wear resistance and ultraviolet resistance in outdoor environments, and are prone to aging, breaking or damage to the protective layer, affecting power generation efficiency and system safety.

Method used

A mixture of ethylene-octene copolymer, low-density polyethylene, white carbon black, flame retardant, maleic anhydride grafted polyethylene, stearic acid, antioxidant and UV absorber was intensively refined at high temperature and passed through twin screws Extrusion granulation to form an insulating and sheathing layer and crosslinked by electron beam irradiation, combining a composite of aluminum hydroxide and magnesium borate whiskers and modified aramid fiber nanosilica filler to enhance the flame retardant of the cable and wear resistance.

Benefits of technology

It significantly improves the weather resistance, aging resistance and wear resistance of photovoltaic cables, extends the service life, and enhances the flame retardant and mechanical properties of the cables.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005059875540000091
    Figure BDA0005059875540000091
Patent Text Reader

Abstract

The invention relates to the technical field of cables, in particular to a photovoltaic cable and a preparation process thereof. An ethylene-octylene copolymer, ethylene propylene diene monomer, low-density polyethylene, white carbon black, a flame retardant, maleic anhydride grafted polyethylene, stearic acid, an antioxidant and an ultraviolet light absorber are mixed, extruded and granulated after banburying to obtain an insulating material, and the insulating material is extruded on the outer side of a cable core to form an insulating layer; an ethylene-octylene copolymer, ethylene propylene diene monomer, low-density polyethylene, white carbon black, a wear-resistant filler, a flame retardant, maleic anhydride grafted polyethylene, calcium stearate, stearic acid, an antioxidant and an ultraviolet light absorber are mixed and internally mixed, then extrusion granulation is performed to obtain a sheath material, the sheath material is extruded on the outer side of the insulating layer to form a sheath layer, and the photovoltaic cable is obtained. The photovoltaic cable prepared by the invention has excellent mechanical property and anti-aging property, and also has excellent flame retardant property, so that the service life of the photovoltaic cable is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of cables, in particular to a photovoltaic cable and a preparation process thereof. Background Art

[0002] Photovoltaic cable is an electrical connection line used in solar photovoltaic power generation systems to transmit the electricity generated by photovoltaic modules to inverters or power grids. With the rapid development of solar photovoltaic power generation technology, the demand for photovoltaic cables is also gradually increasing.

[0003] Traditional power cables have many problems in outdoor environments, such as poor weather resistance, poor abrasion resistance, and insufficient UV resistance. These problems cause photovoltaic cables to age, break, or have their protective layers damaged when exposed to natural environments such as sunlight, rain, and snow. This not only affects the power generation efficiency of the photovoltaic system, but may also have a serious impact on the safety and reliability of the system.

[0004] Therefore, we propose a photovoltaic cable and a preparation process thereof. Summary of the invention

[0005] The object of the present invention is to provide a photovoltaic cable and a preparation process thereof to solve the problems raised in the above background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A process for preparing a photovoltaic cable comprises the following steps:

[0008] Step S1: mixing ethylene-octene copolymer, EPDM rubber, low-density polyethylene, white carbon black, flame retardant, maleic anhydride grafted polyethylene, stearic acid, antioxidant and ultraviolet absorber, kneading at 155-165° C. for 15-30 minutes, and then transferring to a twin-screw extruder for extrusion granulation to obtain an insulating material; extruding the insulating material on the outside of the cable core, cross-linking by electron beam irradiation, and forming an insulating layer;

[0009] Step S2: Ethylene-octene copolymer, EPDM rubber, low-density polyethylene, white carbon black, wear-resistant filler, flame retardant, maleic anhydride grafted polyethylene, calcium stearate, stearic acid, antioxidant and ultraviolet absorber are mixed, kneaded at 155-165° C. for 15-30 min, and then transferred into a twin-screw extruder for extrusion granulation to obtain a sheath material; the sheath material is extruded on the outside of the insulating layer, cross-linked by electron beam irradiation to form a sheath layer, and a photovoltaic cable is obtained.

[0010] Furthermore, the cable core is formed by twisting 12-25 tinned copper conductors.

[0011] Furthermore, the insulating material includes the following components by weight: 20-40 parts of ethylene-octene copolymer, 15-30 parts of EPDM rubber, 10-30 parts of low-density polyethylene, 2-5 parts of white carbon black, 20-40 parts of flame retardant, 3-5 parts of maleic anhydride grafted polyethylene, 1-3 parts of stearic acid, 1-2 parts of antioxidant, and 1-3 parts of ultraviolet absorber.

[0012] Furthermore, the sheath material includes the following components by weight: 20-40 parts of ethylene-octene copolymer, 15-30 parts of EPDM rubber, 10-30 parts of low-density polyethylene, 2-5 parts of white carbon black, 20-40 parts of flame retardant, 4-12 parts of wear-resistant filler, 3-5 parts of maleic anhydride grafted polyethylene, 4-7 parts of calcium stearate, 1-3 parts of stearic acid, 1-2 parts of antioxidant, and 1-3 parts of ultraviolet absorber.

[0013] Furthermore, the preparation method of the flame retardant is as follows:

[0014] Step (1): mixing aluminum chloride hexahydrate and deionized water uniformly, adding sodium hydroxide solution and magnesium borate whiskers, ultrasonically dispersing for 20-40 minutes, adding ethyl acetate dropwise for 30-50 minutes, hydrolyzing at 55-65° C. for 2-4 hours, filtering, washing and drying to obtain a composite;

[0015] Step (2): uniformly mixing the complex, anhydrous ethanol, deionized water and 3-aminopropyltrimethoxysilane, reacting at 55-65° C. for 4-6 hours, filtering, washing and drying to obtain an amino complex;

[0016] Step (3): uniformly mix hexachlorocyclotriphosphazene, triethylamine and tetrahydrofuran, add 4-aminodiphenylamine, heat to 40-50° C., react for 2-3 hours, then add the amino complex, react for 3-5 hours, filter, wash and dry to obtain a flame retardant.

[0017] Furthermore, in the step (1), the mass ratio of aluminum chloride hexahydrate, deionized water, sodium hydroxide solution, magnesium borate whisker and ethyl acetate is 1:(25-35):(8-10):(1.6-1.8):(2.1-2.4), and the concentration of the sodium hydroxide solution is 20-30wt%.

[0018] Furthermore, in step (2), the mass ratio of the composite, anhydrous ethanol, deionized water and 3-aminopropyltrimethoxysilane is 1:(15-20):(2-4):(0.4-0.6).

[0019] Furthermore, in the step (3), the mass ratio of hexachlorocyclotriphosphazene, triethylamine and tetrahydrofuran is 1:(0.5-0.8):(10-12).

[0020] Furthermore, in the step (3), the mass of 4-aminodiphenylamine is 1-2 times the mass of hexachlorocyclotriphosphazene.

[0021] Furthermore, in step (3), the mass of the amination complex is 4-6 times the mass of the hexachlorocyclotriphosphazene.

[0022] In the above technical scheme, aluminum hydroxide is used as an amphoteric hydroxide, which can react with alkali to form metaaluminate, and metaaluminate exists in a reversible chemical equilibrium in an aqueous solution, and then ethyl acetate is used to hydrolyze and consume OH in the water. - , so that the reversible reaction of aluminate is shifted to the right to generate aluminum hydroxide, and the aluminum hydroxide is uniformly coated on the surface of magnesium borate whiskers to obtain a composite; the composite is then modified by 3-aminopropyltrimethoxysilane, and amino groups are introduced to obtain an amino composite; finally, by precisely controlling the proportion of each raw material, the P-Cl bond of hexachlorocyclotriphosphazene and the amino group of the intermediate (4-aminodiphenylamine) of the antioxidant 4010NA undergo nucleophilic substitution reaction, the antioxidant is introduced, and then the amino composite is added to completely react the remaining P-Cl bonds in the system to obtain a halogen-free flame retardant containing N, P, and Si elements.

[0023] Furthermore, the preparation method of the wear-resistant filler is as follows:

[0024] The aramid fiber is dispersed in deionized water to obtain a dispersion, dopamine hydrochloride is added, and the pH value is adjusted to 8.5 with Tris-HCl buffer, and the mixture is stirred for 22-24 hours. After filtering, washing, and drying, the modified aramid fiber is obtained. The modified aramid fiber is ultrasonically dispersed in anhydrous ethanol, ammonia water is added and mixed evenly, and tetraethyl orthosilicate and 1H,1H,2H,2H-perfluoroheptadecantrimethylsilane are added dropwise, and the mixture is completed within 30-40 minutes. The mixture is reacted for 6-8 hours to obtain a wear-resistant filler.

[0025] Furthermore, the concentration of the dispersion is 1-2 mg / mL, and the mass of dopamine hydrochloride is 1-2 times the mass of the aramid fiber.

[0026] Furthermore, the mass ratio of the modified aramid fiber, anhydrous ethanol, ammonia water, tetraethyl orthosilicate and 1H,1H,2H,2H-perfluoroheptadecantrimethyloxysilane is 1:(300-400):(18-20):(8-10):(0.3-0.5).

[0027] In the above technical scheme, through the reaction of aramid fiber and dopamine, dopamine undergoes self-polymerization reaction in a weak alkaline aerobic environment to generate polydopamine, which will be coated on the surface of the aramid fiber, introducing active groups to obtain modified aramid fiber; then nano-silica is in situ grown on its surface by a sol-gel method, and low surface energy modification is performed by 1H,1H,2H,2H-perfluoroheptadecantrimethyloxysilane to obtain a wear-resistant filler with super hydrophobic properties; wherein, the nano-silica particles have high strength, large specific surface area, and extremely strong ultraviolet absorption and infrared reflection characteristics, and the aramid fiber has high strength and wear resistance. Adding it to the sheath material not only enhances the weather resistance and aging resistance of the cable, but also improves the strength and wear resistance of the cable, thereby extending its service life.

[0028] Furthermore, the antioxidant is antioxidant 1010.

[0029] Furthermore, the ultraviolet absorber is UV-326.

[0030] Furthermore, the temperature of the twin-screw extruder is set to: 110-120°C in zone 1, 120-130°C in zone 2, 130-140°C in zone 3, 140-150°C in zone 4, 150-160°C in zone 5, and 145-155°C in zone 6.

[0031] Furthermore, the thickness of the insulating layer is 0.7-1.7 mm.

[0032] Furthermore, the thickness of the sheath layer is 0.8-2.0 mm.

[0033] Furthermore, the process conditions of the electron beam irradiation cross-linking are: irradiation dose of 1.5-2.5 MeV, beam current intensity of 0.5-40 mA, and scanning width of 100-120 cm.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] 1. A photovoltaic cable and its preparation process of the present invention, using a non-uniform nucleation method to coat aluminum hydroxide on the surface of magnesium borate whisker, can increase the dispersibility and stability of aluminum hydroxide, further improve its flame retardant effect in cable materials; at the same time, magnesium borate whisker has the characteristics of light weight, high toughness, wear resistance and good insulation, and can enhance the mechanical properties of the composite; then the composite is organically modified with 3-aminopropyltrimethoxysilane to obtain an amino composite; through the amino compound and the amino group in 4-aminodiphenylamine reacting with the P-Cl bond in hexachlorocyclotriphosphazene, a halogen-free flame retardant containing N, P, Si elements is obtained, and it has an anti-aging effect. Not only can the flame retardancy of the cable be improved, but also its anti-aging property can be improved.

[0036] 2. A photovoltaic cable and a preparation process thereof of the present invention comprises the following steps: aramid fiber and dopamine react, and dopamine undergoes a polymerization reaction in a weak alkaline aerobic environment to generate polydopamine, which is coated on the surface of the aramid fiber, and active groups are introduced to obtain modified aramid fiber; nano-silica is then grown on the surface in situ by a sol-gel method, and low surface energy modification is performed by 1H, 1H, 2H, 2H-perfluoroheptadecantrimethyloxysilane to obtain a wear-resistant filler with super hydrophobic properties; wherein the nano-silica particles have high strength, large specific surface area, and extremely strong ultraviolet absorption and infrared reflection properties, and the aramid fiber has high strength and wear resistance, and adding the nano-silica particles to the sheath material not only enhances the weather resistance and anti-aging ability of the cable, but also improves the strength and wear resistance of the cable, thereby extending its service life. DETAILED DESCRIPTION

[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] In this embodiment, the ethylene-octene copolymer: the brand is Dow POE 8180 from the United States; the ethylene propylene diene monomer rubber: the brand is Sinopec Mitsui EPDM 3092PM; the low-density polyethylene: the brand is Dow LDPE 303E from the United States; the white carbon black: the brand is Wacker V15 from Germany; the maleic anhydride grafted polyethylene: the brand is ZJ-900E; the antioxidant: antioxidant 1010; the ultraviolet absorber: UV-326; the aramid fiber: the brand is DuPont Kevlar 49 from the United States; the magnesium borate whisker: nanometer grade, CAS number is 13703-82-7; the tinned copper conductor: the diameter is 0.5 mm.

[0039] In the following examples and comparative examples, 1 part is equal to 100 g.

[0040] Embodiment 1: A process for preparing a photovoltaic cable, comprising the following processes:

[0041] Step S1: 20 parts of ethylene-octene copolymer, 15 parts of ethylene propylene diene monomer rubber, 10 parts of low-density polyethylene, 2 parts of white carbon black, 20 parts of flame retardant, 3 parts of maleic anhydride grafted polyethylene, 1 part of stearic acid, 1 part of antioxidant and 1 part of ultraviolet absorber are mixed, kneaded at 155° C. for 15 minutes, and then transferred into a twin-screw extruder for extrusion granulation to obtain an insulating material; the insulating material is extruded on the outside of a cable core (formed by twisting 15 tinned copper conductors), and cross-linked by electron beam irradiation (irradiation dose of 2 MeV, beam current intensity of 20 mA, scanning width of 120 cm) to form an insulating layer;

[0042] Step S2: 20 parts of ethylene-octene copolymer, 15 parts of ethylene propylene diene monomer rubber, 10 parts of low-density polyethylene, 2 parts of white carbon black, 20 parts of flame retardant, 4 parts of wear-resistant filler, 3 parts of maleic anhydride grafted polyethylene, 4 parts of calcium stearate, 1 part of stearic acid, 1 part of antioxidant and 1 ultraviolet absorber are mixed, kneaded at 155° C. for 15 minutes, and then transferred into a twin-screw extruder for extrusion granulation to obtain a sheath material; the sheath material is extruded on the outside of the insulating layer, and cross-linked by electron beam irradiation (irradiation dose of 2 MeV, beam current intensity of 20 mA, scanning width of 120 cm) to form a sheath layer to obtain a photovoltaic cable;

[0043] The temperature settings of the twin-screw extruders in step S1 and step S2 are: 120° C. for zone 1, 130° C. for zone 2, 140° C. for zone 3, 150° C. for zone 4, 160° C. for zone 5, and 155° C. for zone 6;

[0044] The preparation method of the flame retardant is as follows:

[0045] Step (1): 15 parts of aluminum chloride hexahydrate and 375 parts of deionized water are mixed uniformly, 120 parts of 20 wt% sodium hydroxide solution and 24 parts of magnesium borate whiskers are added, ultrasonic dispersion is performed for 20 minutes, 31.5 parts of ethyl acetate are added dropwise for 30 minutes, hydrolysis reaction is carried out at 55° C. for 2 hours, and after filtering, washing and drying, a composite is obtained;

[0046] Step (2): 24 parts of the complex, 360 parts of anhydrous ethanol, 48 parts of deionized water and 9.6 parts of 3-aminopropyltrimethoxysilane were mixed evenly, reacted at 55° C. for 4 hours, filtered, washed and dried to obtain an amino complex;

[0047] Step (3): 4 parts of hexachlorocyclotriphosphazene, 2 parts of triethylamine and 40 parts of tetrahydrofuran are mixed evenly, 4 parts of 4-aminodiphenylamine are added, the temperature is raised to 40° C., the reaction is carried out for 2 hours, and then 24 parts of the amino complex are added, the reaction is carried out for 3 hours, and after filtering, washing and drying, a flame retardant is obtained;

[0048] The preparation method of wear-resistant filler is as follows:

[0049] Disperse 4 parts of aramid fiber in deionized water to obtain a 1 mg / mL dispersion, add 4 parts of dopamine hydrochloride, and then use Tris-HCl buffer to adjust the pH value to 8.5, stir for 22 hours, filter, wash and dry to obtain modified aramid fiber; ultrasonically disperse 4 parts of modified aramid fiber in 1200 parts of anhydrous ethanol, add 72 parts of ammonia water and mix evenly, add 32 parts of tetraethyl orthosilicate and 1.2 parts of 1H,1H,2H,2H-perfluoroheptadecantrimethyloxysilane dropwise, add for 30 minutes, react for 6 hours, centrifuge, wash and dry to obtain wear-resistant filler.

[0050] Embodiment 2: A process for preparing a photovoltaic cable, comprising the following processes:

[0051] Step S1: 30 parts of ethylene-octene copolymer, 25 parts of ethylene propylene rubber, 20 parts of low-density polyethylene, 3 parts of white carbon black, 30 parts of flame retardant, 4 parts of maleic anhydride grafted polyethylene, 2 parts of stearic acid, 1.5 parts of antioxidant and 2 parts of ultraviolet absorber are mixed, kneaded at 160° C. for 20 minutes, and then transferred into a twin-screw extruder for extrusion granulation to obtain an insulating material; the insulating material is extruded on the outside of a cable core (composed of 15 tinned copper conductors twisted together), and cross-linked by electron beam irradiation (irradiation dose of 2 MeV, beam current intensity of 20 mA, scanning width of 120 cm) to form an insulating layer;

[0052] Step S2: 30 parts of ethylene-octene copolymer, 25 parts of ethylene propylene rubber, 20 parts of low-density polyethylene, 3 parts of white carbon black, 30 parts of flame retardant, 8 parts of wear-resistant filler, 4 parts of maleic anhydride grafted polyethylene, 6 parts of calcium stearate, 2 parts of stearic acid, 1.5 parts of antioxidant and 2 parts of ultraviolet absorber are mixed, kneaded at 160° C. for 20 minutes, and then transferred into a twin-screw extruder for extrusion granulation to obtain a sheath material; the sheath material is extruded on the outside of the insulating layer, and cross-linked by electron beam irradiation (irradiation dose of 2 MeV, beam intensity of 20 mA, scanning width of 120 cm) to form a sheath layer to obtain a photovoltaic cable;

[0053] The temperature settings of the twin-screw extruders in step S1 and step S2 are: 120° C. for zone 1, 130° C. for zone 2, 140° C. for zone 3, 150° C. for zone 4, 160° C. for zone 5, and 155° C. for zone 6;

[0054] The preparation method of the flame retardant is as follows:

[0055] Step (1): 18 parts of aluminum chloride hexahydrate and 540 parts of deionized water are mixed uniformly, 162 parts of 25 wt% sodium hydroxide solution and 30 parts of magnesium borate whiskers are added, ultrasonic dispersion is performed for 30 minutes, 40 parts of ethyl acetate are added dropwise for 40 minutes, hydrolysis reaction is carried out at 60° C. for 3 hours, and after filtering, washing and drying, a composite is obtained;

[0056] Step (2): 30 parts of the complex, 540 parts of anhydrous ethanol, 90 parts of deionized water and 15 parts of 3-aminopropyltrimethoxysilane were mixed evenly, reacted at 60° C. for 5 hours, filtered, washed and dried to obtain an amino complex;

[0057] Step (3): 6 parts of hexachlorocyclotriphosphazene, 4.2 parts of triethylamine and 66 parts of tetrahydrofuran were mixed evenly, 9 parts of 4-aminodiphenylamine were added, the temperature was raised to 45° C., the reaction was carried out for 2.5 hours, and then 30 parts of the amino complex were added, the reaction was carried out for 4 hours, and after filtering, washing and drying, a flame retardant was obtained;

[0058] The preparation method of wear-resistant filler is as follows:

[0059] 8 parts of aramid fiber were dispersed in deionized water to obtain a 1.5 mg / mL dispersion, 12 parts of dopamine hydrochloride were added, and the pH value was adjusted to 8.5 with Tris-HCl buffer, stirred for 23 hours, filtered, washed, and dried to obtain modified aramid fiber; 8 parts of modified aramid fiber were ultrasonically dispersed in 2800 parts of anhydrous ethanol, 152 parts of ammonia water were added and mixed evenly, 72 parts of tetraethyl orthosilicate and 3.2 parts of 1H,1H,2H,2H-perfluoroheptadecantrimethyloxysilane were added dropwise, the dripping was completed in 35 minutes, the reaction was carried out for 7 hours, and the wear-resistant filler was obtained after centrifugation, washing, and drying.

[0060] Embodiment 3: A process for preparing a photovoltaic cable, comprising the following processes:

[0061] Step S1: 40 parts of ethylene-octene copolymer, 30 parts of ethylene propylene diene monomer rubber, 30 parts of low-density polyethylene, 5 parts of white carbon black, 40 parts of flame retardant, 5 parts of maleic anhydride grafted polyethylene, 3 parts of stearic acid, 2 parts of antioxidant and 3 parts of ultraviolet absorber are mixed, kneaded at 165° C. for 30 minutes, and then transferred into a twin-screw extruder for extrusion granulation to obtain an insulating material; the insulating material is extruded on the outside of a cable core (composed of 15 tinned copper conductors twisted together), and cross-linked by electron beam irradiation (irradiation dose of 2 MeV, beam current intensity of 20 mA, scanning width of 120 cm) to form an insulating layer;

[0062] Step S2: 40 parts of ethylene-octene copolymer, 30 parts of ethylene propylene diene monomer rubber, 30 parts of low-density polyethylene, 5 parts of white carbon black, 40 parts of flame retardant, 12 parts of wear-resistant filler, 5 parts of maleic anhydride grafted polyethylene, 7 parts of calcium stearate, 3 parts of stearic acid, 2 parts of antioxidant and 3 parts of ultraviolet absorber are mixed, kneaded at 165° C. for 30 minutes, and then transferred into a twin-screw extruder for extrusion granulation to obtain a sheath material; the sheath material is extruded on the outside of the insulating layer, and cross-linked by electron beam irradiation (irradiation dose of 2 MeV, beam current intensity of 20 mA, scanning width of 120 cm) to form a sheath layer to obtain a photovoltaic cable;

[0063] The temperature settings of the twin-screw extruders in step S1 and step S2 are: 120° C. for zone 1, 130° C. for zone 2, 140° C. for zone 3, 150° C. for zone 4, 160° C. for zone 5, and 155° C. for zone 6;

[0064] The preparation method of the flame retardant is as follows:

[0065] Step (1): 25 parts of aluminum chloride hexahydrate and 875 parts of deionized water are mixed uniformly, 250 parts of 30 wt% sodium hydroxide solution and 45 parts of magnesium borate whiskers are added, ultrasonic dispersion is performed for 40 minutes, 60 parts of ethyl acetate are added dropwise for 50 minutes, hydrolysis reaction is carried out at 65° C. for 4 hours, and after filtering, washing and drying, a composite is obtained;

[0066] Step (2): 40 parts of the complex, 800 parts of anhydrous ethanol, 160 parts of deionized water and 24 parts of 3-aminopropyltrimethoxysilane are mixed evenly, reacted at 65° C. for 6 hours, filtered, washed and dried to obtain an amino complex;

[0067] Step (3): 10 parts of hexachlorocyclotriphosphazene, 8 parts of triethylamine and 120 parts of tetrahydrofuran are mixed evenly, 20 parts of 4-aminodiphenylamine are added, the temperature is raised to 50° C., the reaction is carried out for 3 hours, and then 40 parts of the amino complex are added, the reaction is carried out for 5 hours, and after filtering, washing and drying, a flame retardant is obtained;

[0068] The preparation method of wear-resistant filler is as follows:

[0069] Disperse 12 parts of aramid fiber in deionized water to obtain a 2 mg / mL dispersion, add 24 parts of dopamine hydrochloride, and then use Tris-HCl buffer to adjust the pH value to 8.5, stir for 24 hours, filter, wash and dry to obtain modified aramid fiber; ultrasonically disperse 12 parts of modified aramid fiber in 4800 parts of anhydrous ethanol, add 240 parts of ammonia water and mix evenly, add 120 parts of tetraethyl orthosilicate and 6 parts of 1H,1H,2H,2H-perfluoroheptadecantrimethyloxysilane dropwise, add for 40 minutes, react for 8 hours, centrifuge, wash and dry to obtain wear-resistant filler.

[0070] Comparative Example 1: A process for preparing a photovoltaic cable, comprising the following processes:

[0071] Compared with Example 2, no wear-resistant filler is added in Comparative Example 1, and other steps are the same as those in Example 2.

[0072] Comparative Example 2: A process for preparing a photovoltaic cable, comprising the following processes:

[0073] Compared with Example 2, the flame retardant in Comparative Example 2 is replaced by aluminum hydroxide, and the other steps are the same as those in Example 2.

[0074] Comparative Example 3: A process for preparing a photovoltaic cable, comprising the following processes:

[0075] Compared with Example 2, in Comparative Example 3, the flame retardant is replaced with a composite, and the other steps are the same as those of Example 2.

[0076] Comparative Example 4: A process for preparing a photovoltaic cable, comprising the following processes:

[0077] The preparation method of the flame retardant is as follows:

[0078] Step (1): 18 parts of aluminum chloride hexahydrate and 540 parts of deionized water are mixed uniformly, 162 parts of 25 wt% sodium hydroxide solution and 30 parts of magnesium borate whiskers are added, ultrasonic dispersion is performed for 30 minutes, 40 parts of ethyl acetate are added dropwise for 40 minutes, hydrolysis reaction is carried out at 60° C. for 3 hours, and after filtering, washing and drying, a composite is obtained;

[0079] Step (2): 30 parts of the complex, 540 parts of anhydrous ethanol, 90 parts of deionized water and 15 parts of 3-aminopropyltrimethoxysilane were mixed evenly, reacted at 60° C. for 5 hours, filtered, washed and dried to obtain an amino complex;

[0080] Step (3): 6 parts of hexachlorocyclotriphosphazene, 4.2 parts of triethylamine and 66 parts of tetrahydrofuran were mixed evenly, 18 parts of 4-aminodiphenylamine were added, the temperature was raised to 45° C., the reaction was carried out for 2.5 hours, and 30 parts of the amino complex were added, the reaction was carried out for 4 hours, and after filtering, washing and drying, a flame retardant was obtained;

[0081] Compared with Example 2, the mass of 4-aminodiphenylamine in Comparative Example 4 is 3 times the mass of hexachlorocyclotriphosphazene; the other steps are the same as those in Example 2.

[0082] Experiment: Take the sheath layers obtained in Examples 1-3 and Comparative Examples 1-4, prepare samples, test their properties respectively and record the test results:

[0083] Anti-aging performance test: dry and wet accelerated aging test was carried out using a xenon lamp aging test chamber with an irradiation intensity of 75W / m 2 , the black mark temperature is 60±2℃, the dry-wet cycle is 100min light + 20min light and spray, the total test time is 720h, and the tensile strength before and after aging is determined according to GB / T 1040 standard. The tensile speed is 100mm / min, and the data is recorded; the hardness before and after aging is determined according to GB / T 531 standard, and the data is recorded.

[0084] The limiting oxygen index of the sample was determined according to GB / T 2406 standard, and the sample size was 125mm×6.5mm×3mm.

[0085] Test Results

[0086]

[0087] According to the data in the above table, we can clearly draw the following conclusions:

[0088] 1. Compared with Examples 1-3, the tensile strength and hardness of the product obtained in Comparative Example 1 are both reduced, indicating that the wear-resistant filler prepared by the present invention can improve the mechanical properties of the sheath layer.

[0089] 2. Compared with Examples 1-3, the products obtained in Comparative Examples 2 and 3 showed a decrease in anti-aging and flame retardancy, which indicates that compared with aluminum hydroxide and the composite, the flame retardant prepared by the present invention has excellent flame retardant properties and anti-aging effect.

[0090] 3. Compared with Examples 1-3, the flame retardancy of the product obtained in Comparative Example 4 is reduced. This is because as the amount of 4-aminodiphenylamine added increases, the remaining P-Cl bonds in the system decrease, resulting in a decrease in the amount of amino complex grafting, which affects the flame retardant effect.

[0091] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0092] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A process for preparing a photovoltaic cable, Features: The steps include: Step S1: mixing ethylene-octene copolymer, EPDM rubber, low-density polyethylene, white carbon black, flame retardant, maleic anhydride grafted polyethylene, stearic acid, antioxidant and ultraviolet absorber, kneading at 155-165° C. for 15-30 minutes, and then transferring to a twin-screw extruder for extrusion granulation to obtain an insulating material; extruding the insulating material on the outside of the cable core, cross-linking by electron beam irradiation, and forming an insulating layer; Step S2: Ethylene-octene copolymer, EPDM rubber, low-density polyethylene, white carbon black, wear-resistant filler, flame retardant, maleic anhydride grafted polyethylene, calcium stearate, stearic acid, antioxidant and ultraviolet absorber are mixed, kneaded at 155-165° C. for 15-30 min, and then transferred into a twin-screw extruder for extrusion granulation to obtain a sheath material; the sheath material is extruded on the outside of the insulating layer, cross-linked by electron beam irradiation to form a sheath layer, and a photovoltaic cable is obtained.

2. A process for preparing a photovoltaic cable according to claim 1, Features: The insulating material comprises the following components by weight: 20-40 parts of ethylene-octene copolymer, 15-30 parts of EPDM rubber, 10-30 parts of low-density polyethylene, 2-5 parts of white carbon black, 20-40 parts of flame retardant, 3-5 parts of maleic anhydride grafted polyethylene, 1-3 parts of stearic acid, 1-2 parts of antioxidant, and 1-3 parts of ultraviolet absorber.

3. A process for preparing a photovoltaic cable according to claim 1, Features: The sheath material comprises the following components by weight: 20-40 parts of ethylene-octene copolymer, 15-30 parts of EPDM rubber, 10-30 parts of low-density polyethylene, 2-5 parts of white carbon black, 20-40 parts of flame retardant, 4-12 parts of wear-resistant filler, 3-5 parts of maleic anhydride grafted polyethylene, 4-7 parts of calcium stearate, 1-3 parts of stearic acid, 1-2 parts of antioxidant, and 1-3 parts of ultraviolet absorber.

4. A process for preparing a photovoltaic cable according to claim 1, Features: The preparation method of the flame retardant is as follows: Step (1): mixing aluminum chloride hexahydrate and deionized water uniformly, adding sodium hydroxide solution and magnesium borate whiskers, ultrasonically dispersing for 20-40 minutes, adding ethyl acetate dropwise for 30-50 minutes, hydrolyzing at 55-65° C. for 2-4 hours, filtering, washing and drying to obtain a composite; Step (2): uniformly mixing the complex, anhydrous ethanol, deionized water and 3-aminopropyltrimethoxysilane, reacting at 55-65° C. for 4-6 hours, filtering, washing and drying to obtain an amino complex; Step (3): uniformly mix hexachlorocyclotriphosphazene, triethylamine and tetrahydrofuran, add 4-aminodiphenylamine, heat to 40-50° C., react for 2-3 hours, then add the amino complex, react for 3-5 hours, filter, wash and dry to obtain a flame retardant.

5. A process for preparing a photovoltaic cable according to claim 1, Features: The preparation method of the wear-resistant filler is as follows: The aramid fiber is dispersed in deionized water to obtain a dispersion, dopamine hydrochloride is added, and the pH value is adjusted to 8.5 using Tris-HCl buffer, and stirred for 22-24 hours. After filtering, washing, and drying, the modified aramid fiber is obtained; The modified aramid fiber is ultrasonically dispersed in anhydrous ethanol, ammonia water is added and mixed evenly, and ethyl orthosilicate and 1H,1H,2H,2H-perfluoroheptadecantrimethylsilane are added dropwise for 30-40 minutes, and the reaction is carried out for 6-8 hours. After centrifugation, washing and drying, a wear-resistant filler is obtained.

6. A process for preparing a photovoltaic cable according to claim 1, Features: The antioxidant is antioxidant 1010.

7. A process for preparing a photovoltaic cable according to claim 1, Features: The ultraviolet absorber is UV-326.

8. A process for preparing a photovoltaic cable according to claim 1, Features: The temperature of the twin-screw extruder is set as follows: zone 1 110-120°C, zone 2 120-130°C, zone 3 130-140°C, zone 4 140-150°C, zone 5 150-160°C, zone 6 145-155°C.

9. A photovoltaic cable obtained according to the preparation process according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Processing technology of sheath material for severe cable of three-generation nuclear power plant

    CN110423392A

  • Hydroxide, zinc borate and whisker synergistic flame-retardant ethylene-vinyl acetate copolymer / low-density polyethylene composite material and preparation method thereof

    CN113512249A

  • Photovoltaic cable and production process thereof

    CN115678156A

  • Flame-retardant photovoltaic cable

    CN118420998A

Cited By

  • Preparation method of aramid nanofiber / polyurethane composite material

    CN120518993A