Composition for hemodialysis shell, raw material for hemodialysis shell as well as preparation method and application of composition and raw material
By using materials such as propylene-ethylene copolymer and block copolymer, hemodialysis shell materials without bisphenol A residue, high transparency, and good anti-beating performance were prepared, which solved the safety hazards of polycarbonate materials and additive precipitation. Problem, suitable for use in the medical field.
Patent Information
- Application Number
- CN202310585893.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-23
AI Technical Summary
The use of polycarbonate in existing hemodialysis shell materials causes bisphenol A residue, which poses safety risks, and there are many types of additives added during the preparation process, which affects the safety and stability of the material.
The composition consisting of propylene-ethylene copolymer, styrene-ethylene-butadiene-styrene block copolymer, antioxidant and light stabilizer is melt extruded at 180-210°C by a twin screw extruder. , prepare hemodialysis shell raw materials, reduce the type and dosage of additives, and improve the safety and stability of the material.
It has achieved hemodialysis shell materials that are free of harmful substances, have high transparency and good anti-beating performance. They are suitable for use in the medical field and solve the safety hazards and additive precipitation problems of polycarbonate materials.
Smart Images

Figure BDA0004243292070000091 
Figure BDA0004243292070000101 
Figure BDA0004243292070000102
Abstract
Description
Technical Field
[0001] The present invention relates to the field of medical equipment, and in particular to a composition for a hemodialysis shell, a raw material for a hemodialysis shell, and a preparation method and application thereof. Background Art
[0002] At present, polymer materials have been widely used in the medical industry. With the aging of the population and the increasing demand for medical technology, the industry's demand for medical-grade plastics will also increase.
[0003] Hemodialysis is one of the important ways for patients with uremia to maintain their lives. Hemodialyzers generally use polycarbonate (PC) as the main material for the dialyzer shell and end caps. Polycarbonate has the advantages of high light transmittance, excellent mechanical properties and low molding yield.
[0004] However, the bisphenol A residue in polycarbonate materials can cause endocrine disorders, induce precocious puberty, cause metabolic disorders and lead to obesity, threatening the health of fetuses and children. Therefore, the EU has banned the production of baby bottles containing the chemical bisphenol A. In addition, polycarbonate materials also have safety risks when used in medical devices such as blood purification.
[0005] Compared with polycarbonate, polypropylene (PP) has the advantages of low price, low processing temperature, and no bisphenol A residue. Therefore, some medical devices previously made of polycarbonate have begun to be replaced by polypropylene.
[0006] CN110903549A discloses a polypropylene composite material and its preparation method and application. In addition to adding polypropylene, the polypropylene composite material provided in the scheme also adds polyethylene, SEBS, paraffin oil, erucic acid amide, several types of antioxidants, toughening agents, etc., to meet the performance requirements of hemodialysis shells. However, because medical and health products are in contact with the human body for a long time, especially for hemodialysis, it is inevitable that byproducts such as auxiliary agents will be precipitated, which will cause harmful effects on the human body. Therefore, the type and amount of auxiliary agents added should be minimized for the raw material formula used in medical and health care. In addition, the products of the composite material will inevitably appear aging and other phenomena when exposed to light sources for a long time, which will accelerate the precipitation of byproducts.
[0007] In summary, it is of great significance to provide a hemodialysis shell raw material that is safe and non-toxic, has excellent mechanical properties, and can meet the performance requirement that the types of raw materials added to the dialysis shell material should not be too many. Summary of the invention
[0008] The purpose of the present invention is to overcome the problems in the prior art that the preparation process of the dialysis shell raw material requires the addition of multiple substances, polycarbonate is used in the preparation process of the dialysis shell, and there is residual bisphenol A.
[0009] In order to achieve the above object, the present invention provides a hemodialysis shell composition on one hand, wherein the hemodialysis shell composition contains the following components which are stored separately or two or more components are stored as a mixture:
[0010] Propylene-ethylene copolymer, styrene-ethylene-butadiene-styrene block copolymer, antioxidant, light stabilizer, transparent agent;
[0011] Wherein, based on the total weight of the composition, the content of the propylene-ethylene copolymer is 91-95wt%, the content of the styrene-ethylene-butadiene-styrene block copolymer is 4-9wt%, the content of the antioxidant is 0.05-0.25wt%, the content of the light stabilizer is 0.05-0.25wt%, and the content of the transparent agent is 0.01-0.25wt%;
[0012] In the propylene-ethylene copolymer, the molar ratio of the monomer provided by ethylene to the monomer provided by propylene is 1:20-95;
[0013] The styrene-ethylene-butadiene-styrene block copolymer is a star-shaped styrene-ethylene-butadiene-styrene block copolymer and / or a linear styrene-ethylene-butadiene-styrene block copolymer.
[0014] The second aspect of the present invention provides a method for preparing a raw material for a hemodialysis shell, the method using the components in the composition for a hemodialysis shell described in the first aspect, comprising:
[0015] (1) mixing propylene-ethylene copolymer, styrene-ethylene-butadiene-styrene block copolymer, antioxidant, light stabilizer and clarifier at 15-28° C. to obtain a mixture;
[0016] (2) melting the mixture on a twin-screw extruder at 180-210° C., extruding and granulating, to obtain a raw material for a hemodialysis shell;
[0017] Wherein, based on the total weight of the propylene-ethylene copolymer, the styrene-ethylene-butadiene-styrene block copolymer, the antioxidant, the light stabilizer and the transparent agent, the amount of the propylene-ethylene copolymer is 91-95wt%, the amount of the styrene-ethylene-butadiene-styrene block copolymer is 4-9wt%, the amount of the antioxidant is 0.05-0.25wt%, the amount of the light stabilizer is 0.05-0.25wt%, and the amount of the transparent agent is 0.01-0.25wt%;
[0018] In the propylene-ethylene copolymer, the molar ratio of the monomer provided by ethylene to the monomer provided by propylene is 1:20-95;
[0019] The styrene-ethylene-butadiene-styrene block copolymer is a star-shaped styrene-ethylene-butadiene-styrene block copolymer and / or a linear styrene-ethylene-butadiene-styrene block copolymer;
[0020] The raw material for the hemodialysis shell has a simple supported beam notched impact strength of 4.5-5 KJ / m at 23°C. 2 .
[0021] The third aspect of the present invention provides a raw material for hemodialysis shell prepared by the method described in the second aspect.
[0022] The fourth aspect of the present invention provides application of the raw material for hemodialysis shell described in the third aspect in the field of medical devices.
[0023] The raw material for hemodialysis shell provided by the technical solution of the present invention solves the potential safety hazard caused by bisphenol A residue in polycarbonate hemodialysis shells. The product has no harmful substance residue, good transparency, high gloss, is resistant to impact and has high strength, and is suitable for use in the medical field. DETAILED DESCRIPTION
[0024] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0025] As mentioned above, the first aspect of the present invention provides a composition for a hemodialysis shell, wherein the composition for a hemodialysis shell contains the following components which are stored separately or in a mixture of two or more:
[0026] Propylene-ethylene copolymer, styrene-ethylene-butadiene-styrene block copolymer, antioxidant, light stabilizer, transparent agent;
[0027] Wherein, based on the total weight of the composition, the content of the propylene-ethylene copolymer is 91-95wt%, the content of the styrene-ethylene-butadiene-styrene block copolymer is 4-9wt%, the content of the antioxidant is 0.05-0.25wt%, the content of the light stabilizer is 0.05-0.25wt%, and the content of the transparent agent is 0.01-0.25wt%;
[0028] In the propylene-ethylene copolymer, the molar ratio of the monomer provided by ethylene to the monomer provided by propylene is 1:20-95;
[0029] The styrene-ethylene-butadiene-styrene block copolymer is a star-shaped styrene-ethylene-butadiene-styrene block copolymer and / or a linear styrene-ethylene-butadiene-styrene block copolymer.
[0030] Preferably, the weight average molecular weight of the star-shaped styrene-ethylene-butadiene-styrene block copolymer is 200,000-280,000; and the weight average molecular weight of the linear styrene-ethylene-butadiene-styrene block copolymer is 200,000-280,000. The inventors found that in this preferred case, the processing performance of the raw material of the hemodialysis shell prepared by the composition and the impact resistance of the product are optimized.
[0031] Preferably, the styrene-ethylene-butadiene-styrene block copolymer is a star-shaped styrene-ethylene-butadiene-styrene block copolymer and a linear styrene-ethylene-butadiene-styrene block copolymer; and
[0032] The weight ratio of the star-shaped styrene-ethylene-butadiene-styrene block copolymer to the linear styrene-ethylene-butadiene-styrene block copolymer is 1:5.
[0033] Preferably, the weight ratio of the star-shaped styrene-ethylene-butadiene-styrene block copolymer to the linear styrene-ethylene-butadiene-styrene block copolymer is 1: 3. The inventors found that in this preferred case, the hemodialysis shell raw material prepared using the composition has good impact resistance and performs well in a drop test.
[0034] Preferably, the propylene-ethylene copolymer has a melt index MFR of 8-25 g / 10 min at 230° C. and a load of 2.16 kg.
[0035] Preferably, the transparent agent is a sorbitol transparent nucleating agent.
[0036] Preferably, the antioxidant is selected from at least one of tetramethyl [(3,5-di-tert-butyl dilauryl thiodipropionate)] methane, thiodiethylene (3,5-di-tert-butyl-4-hydroxyhydrocinnamate), thiobis (2-tert-butyl-5-methylphenol), tris (2,4-di-tert-butyl) phosphite, di-tert-butylphenyl-phosphite, 4,4-thiobis (6-tert-butyl-3-methylphenol) and 2,2-thiobis (6-tert-butyl-4-methylphenol).
[0037] More preferably, the antioxidant is 4,4-thiobis(6-tert-butyl-3-methylphenol).
[0038] Preferably, the light stabilizer is a hindered amine light stabilizer.
[0039] More preferably, the light stabilizer is at least one of bis-2,2,6,6-tetramethylpiperidinol sebacate, poly[1-(2'hydroxyethyl)-2,2,6,6-tetramethyl-4-hydroxypiperidinyl succinate], and hindered amine light stabilizer HS-944.
[0040] More preferably, the light stabilizer is bis-2,2,6,6-tetramethylpiperidinol sebacate.
[0041] As mentioned above, the second aspect of the present invention provides a method for preparing a raw material for a hemodialysis shell, which is carried out using the components in the composition for a hemodialysis shell described in the first aspect, comprising:
[0042] (1) mixing propylene-ethylene copolymer, styrene-ethylene-butadiene-styrene block copolymer, antioxidant, light stabilizer and clarifier at 15-28° C. to obtain a mixture;
[0043] (2) melting the mixture on a twin-screw extruder at 180-210° C., extruding and granulating, to obtain a raw material for a hemodialysis shell;
[0044] Wherein, based on the total weight of the propylene-ethylene copolymer, the styrene-ethylene-butadiene-styrene block copolymer, the antioxidant, the light stabilizer and the transparent agent, the amount of the propylene-ethylene copolymer is 91-95wt%, the amount of the styrene-ethylene-butadiene-styrene block copolymer is 4-9wt%, the amount of the antioxidant is 0.05-0.25wt%, the amount of the light stabilizer is 0.05-0.25wt%, and the amount of the transparent agent is 0.01-0.25wt%;
[0045] In the propylene-ethylene copolymer, the molar ratio of the monomer provided by ethylene to the monomer provided by propylene is 1:20-95;
[0046] The styrene-ethylene-butadiene-styrene block copolymer is a star-shaped styrene-ethylene-butadiene-styrene block copolymer and / or a linear styrene-ethylene-butadiene-styrene block copolymer;
[0047] The raw material for the hemodialysis shell has a simple supported beam notched impact strength of 4.5-5 KJ / m at 23°C. 2 .
[0048] Preferably, the mixing is carried out under stirring conditions and at least meets the following conditions: a rotation speed of 150-200 r / min and a time of 0.5-5 min.
[0049] Preferably, the melting and the extrusion granulation are carried out in a twin-screw extruder, and the main engine speed of the twin-screw extruder is 180-230 r / min.
[0050] As mentioned above, the third aspect of the present invention provides a raw material for hemodialysis shell prepared by the method described in the second aspect.
[0051] As mentioned above, the fourth aspect of the present invention provides the use of the raw material for hemodialysis shell described in the third aspect in the field of medical devices.
[0052] The present invention will be described in detail below by way of examples, but the present invention is not limited thereby.
[0053] In the following examples, unless otherwise specified, all raw materials used are products of Sinopharm Chemical Reagent Co., Ltd.
[0054] Propylene-ethylene copolymer I: purchased from Sinopec Yanshan Petrochemical Company, with a grade of 4912, wherein the molar ratio of the monomer provided by ethylene to the monomer provided by propylene is 1:33, and the melt index MFR at 230°C and a load of 2.16 kg is 12 g / 10 min;
[0055] Propylene-ethylene copolymer II: purchased from Sinopec Yanshan Petrochemical Company, with a grade of 4908, wherein the molar ratio of the monomer provided by ethylene to the monomer provided by propylene is 1:33, and the melt index MFR at 230°C and a load of 2.16 kg is 8 g / 10 min;
[0056] Propylene-ethylene copolymer III: purchased from Sinopec Yanshan Petrochemical Company, brand MPP4016, wherein the molar ratio of the monomer provided by ethylene to the monomer provided by propylene is 1:18; the melt index MFR at 2.16 kg is 20 g / 10 min; the weight average molecular weight is 200,000.
[0057] Homopolymer polypropylene: purchased from Sinopec Yanshan Petrochemical Company, brand k1118, melt index MFR at 2.16 kg is 20 g / 10 min; weight average molecular weight is 200,000.
[0058] Block copolymer I: star-shaped styrene-ethylene-butadiene-styrene block copolymer: weight average molecular weight 220,000, purchased from Yueyang Petrochemical, brand 602;
[0059] Block copolymer II: linear styrene-ethylene-butadiene-styrene block copolymer: weight average molecular weight 220,000, purchased from Asahi Kasei Corporation, brand H1221;
[0060] Block copolymer III: a linear styrene-butadiene-styrene block copolymer with a weight average molecular weight of 330,000, purchased from Sinopec Yanshan Petrochemical Company, with a brand number of 1301;
[0061] Antioxidant: purchased from Sinopec Yanshan Petrochemical Company, model number is antioxidant 168;
[0062] Light stabilizer: purchased from Sinopec Yanshan Petrochemical Company, model number is light stabilizer 622;
[0063] Transparent agent: purchased from Sinopec Yanshan Petrochemical Company, brand name sorbitol transparent agent 8000.
[0064] In the present invention, unless otherwise specified, the normal temperature or room temperature involved in the following examples is 25±5°C.
[0065] In the following examples, each "part by weight" means 100 g unless otherwise specified.
[0066] In the following embodiments, the performance index parameter test standards are as follows:
[0067] Haze injection molding 1mm test: carried out in accordance with standard GB / T 2410-2008;
[0068] Flexural modulus test: carried out in accordance with standard GB / T 9341-2008;
[0069] Yellow index test: carried out in accordance with standard HG / T 3862-2006;
[0070] Simple supported beam notched impact strength (-20℃) test: carried out in accordance with standard GB / T 1043.1-2008;
[0071] Simple supported beam notched impact strength (23°C) test: carried out in accordance with standard GB / T 1043.1-2008;
[0072] Melt mass flow rate test: carried out in accordance with standard GB / T 3682.1-2018;
[0073] Shrinkage test: carried out in accordance with standard GB / T 17037.4-2003.
[0074] Example 1
[0075] This example is used to illustrate the preparation of raw materials for hemodialysis shells using the method provided by the present invention, and is carried out with reference to the parameters and other contents in Table 1, specifically including:
[0076] (1) mixing a propylene-ethylene copolymer (propylene-ethylene copolymer I), a styrene-ethylene-butadiene-styrene block copolymer, an antioxidant, a light stabilizer, and a clarifier for 2 minutes at room temperature and at a stirring speed of 150 r / min to obtain a mixture;
[0077] (2) melting the mixture on a twin-screw extruder at 210° C., adjusting the main engine speed of the extrusion granulation twin-screw extruder to 220 r / min, and performing extrusion granulation to obtain a raw material for hemodialysis shell, named P1;
[0078] Among them, the styrene-ethylene-butadiene-styrene block copolymer is a star-shaped styrene-ethylene-butadiene-styrene block copolymer and a linear styrene-ethylene-butadiene-styrene block copolymer; and the weight ratio of the star-shaped styrene-ethylene-butadiene-styrene block copolymer to the linear styrene-ethylene-butadiene-styrene block copolymer is 1:3.
[0079] Example 2
[0080] This example adopts a method similar to that of Example 1, except that the propylene-ethylene copolymer used is propylene-ethylene copolymer II, and the amount of the substance added is changed. For specific parameters, see Table 1, and a raw material for hemodialysis shell is obtained, named P2.
[0081] Example 3
[0082] This embodiment adopts a method similar to that of Embodiment 1, except that the weight ratio of the star-shaped styrene-ethylene-butadiene-styrene block copolymer to the linear styrene-ethylene-butadiene-styrene block copolymer is 1:4, and the process parameters are changed to obtain a raw material for hemodialysis shell. The specific parameters are shown in Table 1 and are named P3.
[0083] Example 4
[0084] This example adopts a method similar to that of Example 1, except that the styrene-ethylene-butadiene-styrene block copolymers used are all star-shaped styrene-ethylene-butadiene-styrene block copolymers, and a raw material for hemodialysis shell is obtained, which is named P4.
[0085] Comparative Example 1
[0086] This comparative example adopts a method similar to that of Example 1, except that block copolymer III is used instead of styrene-ethylene-butadiene-styrene block copolymer to obtain a raw material for hemodialysis shell, which is named DP1.
[0087] Comparative Example 2
[0088] This comparative example adopts a method similar to that of Example 1, except that propylene-ethylene copolymer III is used instead of propylene-ethylene copolymer I to obtain a raw material for hemodialysis shell, named DP2.
[0089] Comparative Example 3
[0090] This comparative example adopts a method similar to that of Example 1, except that homopolypropylene is used instead of propylene-ethylene copolymer I to obtain a raw material for hemodialysis shell, named DP3.
[0091] Test Example 1
[0092] The melt mass flow rate, flexural modulus, yellowness index, shrinkage rate and other properties of some of the products in the above examples were measured. The test results are shown in Table 2.
[0093] Table 1
[0094]
[0095]
[0096] Table 2
[0097]
[0098] From the above results, it can be seen that the raw material for the hemodialysis shell provided by the present invention does not use polycarbonate, has no harmful substance residue, has good transparency, high gloss, is resistant to impact and has high strength, and is suitable for use in the medical field.
[0099] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection of the present invention.
Claims
1. A composition for hemodialysis shell, characterized in that The hemodialysis shell composition contains the following components which are stored independently or in combination: Propylene-ethylene copolymer, styrene-ethylene-butadiene-styrene block copolymer, antioxidant, light stabilizer, transparent agent; Wherein, based on the total weight of the composition, the content of the propylene-ethylene copolymer is 91-95wt%, the content of the styrene-ethylene-butadiene-styrene block copolymer is 4-9wt%, the content of the antioxidant is 0.05-0.25wt%, the content of the light stabilizer is 0.05-0.25wt%, and the content of the transparent agent is 0.01-0.25wt%; In the propylene-ethylene copolymer, the molar ratio of the monomer provided by ethylene to the monomer provided by propylene is 1:20-95; The styrene-ethylene-butadiene-styrene block copolymer is a star-shaped styrene-ethylene-butadiene-styrene block copolymer and / or a linear styrene-ethylene-butadiene-styrene block copolymer.
2. The composition according to claim 1, wherein The weight average molecular weight of the star-shaped styrene-ethylene-butadiene-styrene block copolymer is 200,000-280,000; and The weight average molecular weight of the linear styrene-ethylene-butadiene-styrene block copolymer is 200,000-280,000.
3. The composition according to claim 1 or 2, wherein The styrene-ethylene-butadiene-styrene block copolymer is a star-shaped styrene-ethylene-butadiene-styrene block copolymer and a linear styrene-ethylene-butadiene-styrene block copolymer; and The weight ratio of the star-shaped styrene-ethylene-butadiene-styrene block copolymer to the linear styrene-ethylene-butadiene-styrene block copolymer is 1:
5.
4. The composition according to any one of claims 1 to 3, wherein The propylene-ethylene copolymer has a melt index MFR of 8-25 g / 10 min at 230° C. and a load of 2.16 kg; and / or The transparent agent is a sorbitol transparent nucleating agent.
5. The composition according to any one of claims 1 to 4, wherein The antioxidant is selected from at least one of tetramethyl [(3,5-di-tert-butyl dilauryl thiodipropionate)] methane, thiodiethylene (3,5-di-tert-butyl-4-hydroxyhydrocinnamate), thiobis (2-tert-butyl-5-methylphenol), tris (2,4-di-tert-butyl) phosphite, di-tert-butylphenyl-phosphite, 4,4-thiobis (6-tert-butyl-3-methylphenol) and 2,2-thiobis (6-tert-butyl-4-methylphenol); Preferably, the antioxidant is 4,4-thiobis(6-tert-butyl-3-methylphenol).
6. The composition according to any one of claims 1 to 5, wherein The light stabilizer is a hindered amine light stabilizer; Preferably, the light stabilizer is at least one of bis-2,2,6,6-tetramethylpiperidinol sebacate, poly[1-(2'hydroxyethyl)-2,2,6,6-tetramethyl-4-hydroxypiperidinyl succinate], and hindered amine light stabilizer HS-944; Preferably, the light stabilizer is bis-2,2,6,6-tetramethylpiperidinol sebacate.
7. A method for preparing a raw material for a hemodialysis shell, characterized in that: The method is carried out using the components in the hemodialysis shell composition according to any one of claims 1 to 6, comprising: (1) mixing propylene-ethylene copolymer, styrene-ethylene-butadiene-styrene block copolymer, antioxidant, light stabilizer and clarifier at 15-28° C. to obtain a mixture; (2) melting the mixture on a twin-screw extruder at 180-210° C., extruding and granulating, to obtain a raw material for a hemodialysis shell; Wherein, based on the total weight of the propylene-ethylene copolymer, the styrene-ethylene-butadiene-styrene block copolymer, the antioxidant, the light stabilizer and the transparent agent, the amount of the propylene-ethylene copolymer is 91-95wt%, the amount of the styrene-ethylene-butadiene-styrene block copolymer is 4-9wt%, the amount of the antioxidant is 0.05-0.25wt%, the amount of the light stabilizer is 0.05-0.25wt%, and the amount of the transparent agent is 0.01-0.25wt%; In the propylene-ethylene copolymer, the molar ratio of the monomer provided by ethylene to the monomer provided by propylene is 1:20-95; The styrene-ethylene-butadiene-styrene block copolymer is a star-shaped styrene-ethylene-butadiene-styrene block copolymer and / or a linear styrene-ethylene-butadiene-styrene block copolymer; The raw material for the hemodialysis shell has a simple supported beam notched impact strength of 4.5-5 KJ / m at 23°C. 2 .
8. The method according to claim 7, wherein: The mixing is carried out under stirring conditions and at least meets the following conditions: the rotation speed is 150-200 r / min and the time is 0.5-5 min; and / or The melting and the extrusion granulation are carried out in a twin-screw extruder, and the main engine speed of the twin-screw extruder is 180-250r / min.
9. A raw material for hemodialysis shell prepared by the method according to claim 7 or 8.
10. Use of the raw material for hemodialysis shell according to claim 9 in the field of medical devices.
Citation Information
Patent Citations
Polyolefin composition
CN111051417A
Polypropylene / thermoplastic elastomer blend as well as preparation method and application thereof
CN112708192A
Polypropylene composition, polypropylene material and preparation method and application thereof
CN114907643A
Propylene-based resin composition for medical member, and medical member
JP2014212916A
Polyolefin composition
US20200239676A1