Preparation method and application of polymerizable eutectic gel conductive elastomer based on supramolecular crosslinking

Through the preparation of supramolecular cross-linked polymerizable eutectic gel conductive elastomer, the problem of ionic conductive elastomer in the prior art is solved, and the high level of the flexible sensor is achieved Mechanical strength, toughness and recyclability improve the application reliability and environmental protection of the equipment.

CN119019800APending Publication Date: 2024-11-26HEFEI UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411281533.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing hydrogel-based ionic conductive elastomers are prone to failure in extreme environments, and their alternative materials such as ionic liquids are complex and costly, and have insufficient environmental protection, resulting in insufficient application reliability and environmental protection in flexible electronic devices.

Method used

The preparation method of polymerizable eutectic gel conductive elastomer with supramolecular crosslinking is adopted, and the photoinduced radical polymerization method is used to use acrylic acid, choline chloride, aluminum nitrate nohydrate and amino-terminated hyperbranched aramid groups. PDES/Al/AF-AP conductive elastomer with excellent ductility, toughness and recyclability were prepared by ultraviolet curing crosslinking reaction.

Benefits of technology

It has excellent mechanical strength, toughness and conductivity in flexible sensors, and material recyclability is achieved through reversible supramolecular interaction, improving the application reliability and environmental protection of the equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019800A_ABST
    Figure CN119019800A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a polymerizable eutectic gel conductive elastomer based on supramolecular crosslinking, and relates to the technical field of preparation of flexible conductive elastomers. The preparation method comprises the following steps: firstly, mixing acrylic acid with choline chloride, then adding aluminum nitrate nonahydrate to fully dissolve, then adding amino-terminated hyperbranched aramid and a photoinitiator, uniformly dispersing to prepare a precursor solution, and finally preparing the ionic conductive elastomer PDES / Al / AF-AP through a photocuring cross-linking reaction. The ionic conductive elastomer shows excellent ductility and enhanced mechanical strength, and maintains good conductivity and stability. Benefited from the supramolecular action of hydrogen bonds and ion coordination, the elastomer has recoverability, and step-by-step recovery of the amino-terminated hyperbranched aramid filler and the gel elastomer can be realized through the processes of dissolution, dispersion, centrifugation and casting. In addition, due to the conductivity and the stability of the material, the material shows important application potential in flexible sensing devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of flexible conductive elastomer preparation, and in particular to a method for preparing a polymerizable low eutectic gel conductive elastomer based on supramolecular cross-linking. At the same time, the present invention also covers the application and recycling of the conductive elastomer. Background Art

[0002] In recent years, ion-conductive elastomers have shown wide application potential in the field of flexible electronics (such as sensors, batteries, supercapacitors and soft robots). Especially in flexible wearable electronic devices, hydrogel-based ion conductors have attracted much attention due to their excellent biocompatibility and flexibility. However, this type of material has deficiencies in environmental adaptability, especially under extreme conditions, where evaporation or freezing of water can easily lead to functional failure, limiting its reliability in practical applications. For this reason, ion gels have become a research hotspot. They replace the aqueous phase with ionic liquids, have non-volatility, high stability and excellent conductivity, and become ideal hydrogel substitutes. However, the preparation of ionic liquids is usually more complicated than that of organic solvents and has higher costs. In addition, its environmental friendliness also depends on the structure of cations and anions in the ionic liquids, which means that ionic liquids are not completely "green" materials.

[0003] To solve the above problems, deep eutectic solvents (DES) have become a new opportunity for the development of ionic conductors because of their greenness, non-volatility, easy preparation, low cost and wide operating temperature range. Recently, polymerizable deep eutectic solvents (PDES) containing acrylic acid or methacrylic acid groups have been used to improve the environmental stability and conductive properties of conductive elastomers. For example, Wang et al. prepared elastomers based on PDES (acrylic acid / choline chloride, AA / ChCl) and liquid metal nanodroplets, which have high strain (2600%) but low tensile strength (0.13MPa) [Advanced Materials, 2023, 35(20), 2211731]. In contrast, Lu et al. developed an ionic conductor based on PDES, combined with AA / ChCl and monomers derived from vanilla, showing good strength (1.48MPa), but limited strain capacity (500%) [Chemical Engineering Journal, 2021, 425, 130652].

[0004] Therefore, although PDES-based elastomers have certain advantages, the thermoplastic polyacrylic acid material obtained by in-situ photopolymerization is relatively soft at room temperature, and its mechanical strength and toughness are still significantly different from those of traditional elastomer materials. In addition, in the poly-eutectic-based conductive elastic system, its recovery after repeated stretching is insufficient, resulting in poor sensing stability, which needs to be further improved. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention proposes an innovative, green and sustainable one-pot synthesis method, namely, a preparation method and application of a polymerizable low-eutectic gel conductive elastomer based on supramolecular cross-linking. The prepared elastomer has excellent ductility, toughness, recyclability and outstanding sensing performance, showing application potential as a flexible sensor.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing a polymerizable low-melting gel conductive elastomer based on supramolecular cross-linking, using a photo-initiated free radical polymerization method, first, acrylic acid (AA) and choline chloride (ChCl) are mixed to form a transparent solution (DES), a non-covalent cross-linking agent aluminum nitrate nonahydrate (Al(NO3)3·9H2O) is added, and it is fully dissolved by ultrasound; then, amino-terminated hyperbranched aramid (AF-AP) and a photoinitiator (I2959) are added and dispersed and mixed uniformly; finally, the obtained mixture is transferred to a mold, and a polymerizable low-melting gel conductive elastomer based on supramolecular cross-linking is prepared by a photocuring cross-linking reaction, namely, PDES / Al / AF-AP conductive elastomer.

[0008] As a preferred technical solution of the present invention, the preparation method steps are as follows:

[0009] Step 1: mixing choline chloride (ChCl) and acrylic acid (AA) in a certain molar ratio to form a mixture; heating and stirring the mixture to obtain a solution A that can remain clear and transparent at room temperature;

[0010] Step 2: weigh an appropriate amount of aluminum nitrate nonahydrate (Al(NO3)3·9H2O) and mix it with solution A, and perform ultrasonic treatment to form solution B;

[0011] Step 3: Weigh an appropriate amount of amino-terminated hyperbranched aramid (AF-AP) and mix with solution B, stir and disperse evenly, then add the photoinitiator (I2959), and stir again to form a precursor solution C;

[0012] Step 4: Pour the obtained precursor solution C into a polytetrafluoroethylene mold and place it under ultraviolet light for curing, thereby preparing a PDES / Al / AF-AP conductive elastomer.

[0013] As a further preferred technical solution of the present invention, in the preparation method:

[0014] The molar ratio of choline chloride (ChCl) to acrylic acid (AA) is 1:1.5-2.5, the mass ratio of solution A to aluminum nitrate nonahydrate (Al(NO3)3·9H2O) is 100-200:1, the mass ratio of solution A to amino-terminated hyperbranched aramid (AF-AP) is 100:0.1-1, and the mass ratio of solution A to photoinitiator (I2959) is 500-1000:1.

[0015] In step 1, the mixture is heated and stirred at 80-100° C. for 1-5 h.

[0016] In step 3, after adding amino-terminated hyperbranched aramid (AF-AP) and initiator, stir for 10 to 30 minutes respectively to achieve uniform mixing, the stirring temperature is 25 to 30° C., and the stirring speed is 300 to 400 rpm.

[0017] In step 4, the photocuring cross-linking reaction is cured under ultraviolet light with a wavelength of 365 nm for 60 to 600 seconds, and the reaction temperature is 25 to 30°C.

[0018] The polymerizable low-eutectic gel conductive elastomer based on supramolecular cross-linking prepared by the present invention can be applied in wearable sensors for detecting human body movements.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0020] 1. The present invention uses amino-terminated hyperbranched aramid (AF-AP) and metal (Al) ion-modified PDES to make a precursor, and then uses in-situ photopolymerization technology to prepare an ion-conductive elastomer (PDES / Al / AF-AP) based on amino-functionalized aramid and ion-synergistic non-covalent reinforcement. This ion-conductive elastomer exhibits excellent ductility and enhanced mechanical strength, and maintains good conductivity and stability. Thanks to the supramolecular effects of hydrogen bonding and ion coordination, this elastomer is recyclable, and the amino-terminated hyperbranched aramid filler and gel elastomer can be recycled step by step through the dissolution-dispersion-centrifugation-casting process.

[0021] 2. The polymerizable low-melting gel conductive elastomer based on supramolecular cross-linking prepared by the present invention has important application potential in flexible sensor devices due to its conductivity and stability, and is particularly suitable for the field of human motion monitoring.

[0022] 3. The preparation method proposed in the present invention is simple, environmentally friendly, and low-cost, and solves the deficiencies of existing conductive elastomers in terms of mechanical properties and recyclability. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1This is a flow chart for the preparation of the polymerizable eutectic gel conductive elastomer based on supramolecular cross-linking proposed in the present invention.

[0024] Figure 2 For preparing each elastomer PDES / Al in Examples 4 to 8 0.81 / AF-AP 0.1 PDES / Al 0.81 / AF-AP 0.3 PDES / Al 0.81 / AF-AP 0.5 PDES / Al 0.81 / AF-AP 0.75 PDES / Al 0.81 / AF-AP1 stress-strain curve (2a), tensile and toughness comparison (2b), and performance comparison with other works (2c); Example 6 prepared elastomer tensile recovery image at 500% strain (2d); image of lifting heavy objects (2e); digital image under torsion and knotting (2f); loading and unloading stress-strain curves under different tensile strains (2g) and corresponding dissipated energy (U hys ) and toughness values ​​(2h) and cyclic loading and unloading stress-strain curves (2i) at different rest times and 100% strain, the corresponding U hys and recovery of peak stress (2j).

[0025] Figure 3 EDS (3a), infrared spectrum (3b), and X-ray photoelectron spectroscopy XPS (3c-3f) of the elastomer prepared in Example 6.

[0026] Figure 4 The recycling mechanism diagram (4a), recycling flow chart (4b, 4c) and recovery rate comparison (4d) of the elastomer prepared by the present invention are shown.

[0027] Figure 5 The relationship between the relative resistance change and strain of the elastomer prepared in Example 2 (5a), the relative resistance change of the elastomer prepared in Example 6 within a large strain range (10-250%) (5b), repeated stretching and release experiments (5c), and the measurement factor of the strain sensor (5d) are prepared. The elastomer used in Example 6 is used to monitor the human body's movement process and the strain sensing performance diagram (5e), ​​as well as the self-healing ability detection curve (5f). DETAILED DESCRIPTION

[0028] The present invention is further described in detail below in conjunction with embodiments and drawings.

[0029] Example 1

[0030] Preparation of polymerizable low eutectic solvent DES: Choline chloride and acrylic acid were mixed in a molar ratio of 1:2, and the mixture was heated and stirred at 90° C. for 3 h in a round-bottom flask to obtain a uniform clear and transparent solution DES, and the prepared DES was sealed and waited for the next step.

[0031] Preparation of PDES: 16 mg of photoinitiator (I2959) was added to 10 g of the obtained clear and transparent solution, and after magnetic stirring, the solution was transferred to a polytetrafluoroethylene mold, and placed in a UV curing machine for irradiation and curing for 90 seconds to obtain PDES. The magnetic stirring temperature was 25°C, the stirring speed was 300 rpm, and the stirring time was 10 minutes.

[0032] Example 2

[0033] Preparation of polymerizable low eutectic solvent DES: Choline chloride and acrylic acid were mixed in a molar ratio of 1:2, and the mixture was heated and stirred at 90° C. for 3 h in a round-bottom flask to obtain a uniform clear and transparent solution DES, and the prepared DES was sealed and waited for the next step.

[0034] Preparation of prepolymer solution: 81 mg of aluminum nitrate nonahydrate (Al(NO3)3·9H2O) was added to 10 g of the prepared clear transparent solution, and ultrasonic dispersion was performed uniformly for 30 min.

[0035] PDES / Al 0.81 Preparation: 16 mg of photoinitiator (I2959) was added and stirred evenly by magnetic force to obtain an elastomer precursor solution, and the elastomer precursor solution was transferred to a polytetrafluoroethylene mold, and then placed in a UV curing machine for irradiation and curing for 90 seconds to obtain PDES / Al 0.81 The temperature of magnetic stirring was 25°C, the stirring speed was 300 rpm, and the stirring time was 10 min.

[0036] Example 3

[0037] Preparation of polymerizable low eutectic solvent DES: Choline chloride and acrylic acid were mixed in a molar ratio of 1:2, and the mixture was heated and stirred at 90° C. for 3 h in a round-bottom flask to obtain a uniform clear and transparent solution DES, and the prepared DES was sealed and waited for the next step.

[0038] Preparation of prepolymer solution: 50 mg of amino-terminated hyperbranched aramid (AF-AP) was added to 10 g of the prepared clear transparent solution and stirred evenly by magnetic stirring at a temperature of 25° C., a stirring speed of 300 rpm, and a stirring time of 30 min.

[0039] PDES / AF-AP 0.5Preparation: 16 mg of photoinitiator (I2959) was added and stirred evenly by magnetic force to obtain an elastomer precursor solution, and the elastomer precursor solution was transferred to a polytetrafluoroethylene mold, and then placed in a UV curing machine for irradiation and curing for 90 seconds to obtain PDES / AF-AP 0.5 The temperature of magnetic stirring was 25°C, the stirring speed was 300 rpm, and the stirring time was 10 min.

[0040] Example 4

[0041] Preparation of polymerizable low eutectic solvent DES: Choline chloride and acrylic acid were mixed in a molar ratio of 1:2, and the mixture was heated and stirred at 90° C. for 3 h in a round-bottom flask to obtain a uniform clear and transparent solution DES, and the prepared DES was sealed and waited for the next step.

[0042] Preparation of prepolymer solution: 81 mg of aluminum nitrate nonahydrate (Al(NO3)3·9H2O) was added to 10 g of the obtained clear transparent solution, and after ultrasonic dispersion, 10 mg of amino-terminated hyperbranched aramid (AF-AP) was added and magnetic stirring was performed. The magnetic stirring temperature was 25°C, the stirring speed was 300 rpm, the ultrasonic time was 30 min, and the stirring time was 30 min.

[0043] PDES / Al 0.81 / AF-AP 0.1 Preparation: 16 mg of photoinitiator (I2959) was added and stirred evenly by magnetic force to obtain an elastomer precursor solution, and the elastomer precursor solution was transferred to a polytetrafluoroethylene mold, and then placed in a UV curing machine for irradiation and curing for 90 seconds to obtain PDES / Al 0.81 / AF-AP 0.1 The temperature of magnetic stirring was 25°C, the stirring speed was 300 rpm, and the stirring time was 10 min.

[0044] Example 5

[0045] The preparation steps are basically the same as those in Example 4, except that the added amino-terminated hyperbranched aramid (AF-AP) is 30 mg in mass, and PDES / Al is prepared. 0.81 / AF-AP 0.3 .

[0046] Example 6

[0047] The preparation steps are basically the same as those in Example 4, except that the added amino-terminated hyperbranched aramid (AF-AP) is 50 mg in mass, and PDES / Al is prepared. 0.81 / AF-AP 0.5 .

[0048] Example 7

[0049] The preparation steps are basically the same as those in Example 4, except that the added amino-terminated hyperbranched aramid (AF-AP) is 75 mg in mass, and PDES / Al is prepared. 0.81 / AF-AP 0.75 .

[0050] Example 8

[0051] The preparation steps are basically the same as those in Example 4, except that the added amino-terminated hyperbranched aramid (AF-AP) has a mass of 100 mg. 0.81 / AF-AP1.

[0052] Figure 1 The one-pot synthetic strategy for the present elastomer is shown. In this DES system, the components participate in non-covalent supramolecular crosslinking to form a conductive elastomer characterized by hydrogen bonding and ionic interactions. Choline chloride (ChCl) acts as a hydrogen bond acceptor (HBA), while acrylic acid (AA) acts as both a hydrogen bond donor (HBD) and a polymerizable monomer.

[0053] Performance test of PDES / Al / AF-AP conductive elastomer prepared in Examples 1 to 8:

[0054] (1) EDS elemental analysis: Energy dispersive spectroscopy (EDS) measurements were performed using an electron microscope (Guoyi Quantum 3200).

[0055] (2) X-ray photoelectron spectroscopy: X-ray photoelectron spectroscopy (XPS) was measured using an X-ray photoelectron spectrometer (Thermo Scientific ESCALAB250Xi).

[0056] (3) Infrared test: recorded using a Nicolet spectrometer (Thermo Nicolet, USA) with a scanning wavelength range of 400 to 4000 cm -1 .

[0057] (4) Mechanical property test: Mechanical tests were carried out on different elastomers using Electronic universal testing machines (TH-8201S, Suzhou Tophung Machine Equipment Co., Ltd., China) at a tensile speed of 1 mm / s. The prepared samples were made into dumbbell-shaped specimens with a total length of 5 cm, an outer width of 8 mm, a narrow length of 1.5 cm, a width of 4 mm, and a thickness of ≈1 mm. The cyclic test was to continuously stretch the gel to 100% strain for 100 consecutive cycles. The test environment temperature was 25°C and the relative humidity was 30% to 35%.

[0058] (5) Resistance-time signal measurement: The electrical properties of the conductive elastomer were measured using a digital bridge (LCR 302, China) in an environment with a temperature of 25°C and a relative humidity of 30% to 35%.

[0059] (6) Optical image capture: Use a camera to capture an optical image of the conductive elastomer.

[0060] Through mechanical testing, the mechanical properties of the supramolecular elastomer prepared by the present invention are shown in the following table:

[0061] Table 1 Mechanical properties of PDES / Al / AF-AP conductive elastomers prepared in Examples 4 to 8

[0062]

[0063] Table 1 shows the mechanical properties data of the PDES / Al / AF-AP conductive elastomers prepared in Examples 4 to 8. Figure 2 a and b are the stress-strain curves (2a) and tensile and toughness comparison diagrams (2b) of each conductive elastomer in room temperature environment. The stress-strain curve of the elastomer shows that the tensile stress (tensile strength) and strain (elongation at break) increase with the increase of AF-AP content. When AF-AP increases from 0.1wt% to 0.5wt%, the tensile stress increases from 4.71±0.23MPa to 6.69±0.06MPa, and the strain increases from 1184±66.00% to 7218±135.87%. However, the excessive introduction of AF-AP will lead to agglomeration, resulting in poor improvement effect and even reduce the mechanical properties of the elastomer. When the AF-AP content increases from 0.1% to 1%, the toughness of the elastomer initially increases and then decreases. When the AF-AP content reaches 0.5% (275.7±16.23MJ*m -3 ) toughness reaches its peak. Therefore, we chose PDES / Al with excellent comprehensive mechanical properties. 0.81 / AF-AP 0.5 The elastomer (prepared in Example 6) was further studied. It is worth noting that PDES / Al 0.81 / AF-AP 0.5 The toughness is about PDES / Al 0.81 / AF-AP 0.1 (Prepared in Example 4) is 8 times tougher.

[0064] Figure 2 c is a performance comparison chart of Example 6 and other works. The tensile strength and elongation at break are better than most reported DES-based copolymers and elastomers. The sources of the literature in the figure are:

[0065] Ref.1:D-gluconic acetal gelator-based supramolecular–Polymer dualnetwork eutectogels for high performance temperature,strain,and pressuresensors.

[0066] Ref.2:Tough Liquid-Free Ionic Conductive Elastomers with RobustAdhesion and Self-Healing Properties for Ionotronic Devices

[0067] Ref.3:Tough and Ultrastretchable Liquid-Free Ion ConductorStrengthened by Deep Eutectic Solvent Hydrolyzed Cellulose Microfibers

[0068] Ref.4:A novel conductive composite gel based on polyvinyl alcohol / polymerizabledeep eutectic solvent with superior tear resistance,tensileproperties and recyclability

[0069] Ref.5:Highly stretchable,self-healing,and adhesive polymericeutectogel enabled by hydrogen-bond networks for wearable strain sensor

[0070] Ref.6:Freeze-Resistant,Conductive,and Robust Eutectogels of MetalSalt-Based Deep Eutectic Solvents with Poly(vinyl alcohol

[0071] Ref.7:Low-Molecular-Weight Supramolecular-Polymer Double-NetworkEutectogels for Self-Adhesive and Bidirectional Sensors

[0072] Ref.8:A cellulose-based self-healing composite eutectogel with reversibility and recyclability for multi-sensing)

[0073] Ref.9:Peptide-enhanced tough,resilient and adhesive eutectogels forhighly reliable strain / pressure sensing under extreme conditions

[0074] Ref.10:Polymerizabledeep eutectic solvent-based mechanically strong and ultra-stretchable conductive elastomers for detecting human motions

[0075] Figure 2 d shows that the conductive elastomers prepared in Example 6 can quickly recover their original shape under a tensile strain of 500%, indicating that they have excellent self-healing properties. Figure 2 e and f are optical photographs showing that the conductive elastomer prepared in Example 6 can withstand good deformation, such as twisting and knotting (2f), and a sample of about 0.6 g can lift an object about 8300 times heavier than itself (2e). Figure 2 g, h are the stress-strain curves (2g) of the conductive elastomer prepared in Example 6 under different tensile strains and the corresponding U hys When the strain increases to 900%, the dissipated energy gradually increases from 1.802 to 5.587 MJ*m -3 This confirms that as the strain increases, the supramolecular network is continuously destroyed to dissipate energy and then recombined through a large number of physical interactions, with excellent recovery properties. Figure 2i and j are the cyclic loading and unloading stress-strain curves (2i) of the conductive elastomer prepared in Example 6 at different rest times with 100% strain, and the corresponding U hys and recovery of peak stress (2j). The self-recovery behavior of the elastomer was tested by applying a dwell time between two consecutive loading and unloading cycles. It is clear that the hysteresis loop becomes larger and the tensile stress becomes larger with increasing rest time. After a dwell time of only 3 min, 93.6% of the dissipated energy is recovered and nearly 100% of the stress is recovered.

[0076] Figure 3 a is the energy spectrum (EDS) of the conductive elastomer prepared in Example 6, showing that AF-AP and Al 3+ The distribution in the elastomer is uniform. The CHO element is large in number and evenly distributed, the N element comes from the nitrate ions of AF-AP and aluminum nitrate nonahydrate, and the Al element comes from aluminum nitrate nonahydrate. Figure 3 b is the FTIR infrared spectrum of the conductive elastomer prepared in Example 6 (compared with the elastomers prepared in Examples 1 to 3). According to the results, compared with the elastomer added with Al and aramid, the conductive elastomer prepared in Example 6 has no obvious difference in composition and structure. Figure 3 c~f are the XPS of the conductive elastomer prepared in Example 6. It can be seen from the figure that the main elements of the elastomer are C, N, O and Cl. As shown in the high-resolution XPS spectrum, the C1s spectrum of the elastomer has three peaks at 284.8, 286.6, and 289.0, corresponding to the CC group, CO / C-OH group, and C=O group, respectively. The O1s spectrum in the figure shows two peaks at 531.6 and 533.1 eV, corresponding to the two main peaks of the C=O and CO groups, respectively. The N1s spectrum in the figure shows two peaks at 399.3 and 402.2 eV, corresponding to the two main peaks of the N-(C=O)- and NO groups, respectively.

[0077] Figure 4 a is a diagram showing the recovery mechanism of the conductive elastomer prepared in Example 6, showing the reversible supramolecular interaction in the conductive elastomer. Figure 4 b is a schematic diagram of the dissolution process of the elastomer. The damaged or fatigued elastomer was placed in water and stirred at room temperature for 6 h to completely dissolve. Figure 4 c is the recovery of AF-AP and PDES / Al from the conductive elastomer prepared in Example 6. The dissolved solution was then centrifuged at 10,000 rpm, the supernatant was cast into a polytetrafluoroethylene mold, and dried in an oven at 35° C. for 24 h to form a regenerated elastomer after water evaporation. Figure 4d is the recovery rate of AF-AP and PDES / Al from the conductive elastomer prepared in Example 6. The aramid powder obtained by centrifugation was washed with deionized water, filtered and dried. The results showed that the high recovery rate of AF-AP was 90.2%, and the recovery rate of PDES / Al was 90.2%. 0.81 The high recovery rate was 88.3%. The stirring process destroyed the hydrogen bonds and ionic coordination bonds, allowing the PAA chains to reversibly unwind, thereby dispersing or dissolving the AF-AP and polymer chains in water. By evaporating the water, the supramolecular interactions and entanglement of the PAA chains were restored.

[0078] Figure 5 a is the relationship between the relative resistance change and strain of the elastomer prepared in Example 2. The ΔR / R0 of the elastomer under strain (50%, 100%, 200%, 300%, 400% and 500%) was tested, and it was found that its stability was very poor, and it dropped very significantly after only 5 repetitions, indicating that its recovery after cyclic stretching was poor. Figure 5 b and c show the relative resistance change of the conductive elastomer prepared in Example 6 over a large strain range (10-250%). The elastomer continuously extends from 10% to 250%, and ΔR / R0 increases steadily from 13.9% to 551.4%, respectively. After releasing the applied strain, the supramolecular PDES ion elastomer quickly returns to its initial resistance, and ΔR / R0 is close to zero. During repeated stretching and release, ΔR / R0 shows excellent consistency at different strain levels, indicating that the elastomer's sensitivity to strain has remarkable stability. Figure 5 d is the measurement factor (GF) of the conductive elastomer strain sensor prepared in Example 6. When 0-100% strain is 1.51, 100-300% strain is 2.53, 300-500% strain is 4.00, and 500-700% strain is 4.52, the high sensitivity of these elastomers is highlighted. Figure 5 e is the relative resistance change of the finger bending of the conductive elastomer prepared in Example 6, showing that it can be effectively used as a wearable sensor for human joints, facilitating accurate monitoring of human movement. Figure 5 f is a study of the electrical self-healing ability of the conductive elastomer prepared in Example 6, showing the real-time resistance change of the elastomer during the cut-healing cycle. Once cut, the resistance of the elastomer immediately becomes infinite; after reconnection, the resistance immediately returns to the original value.

[0079] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a polymerizable eutectic gel conductive elastomer based on supramolecular cross-linking, using a photo-initiated free radical polymerization method, characterized in that: First, acrylic acid (AA) and choline chloride (ChCl) were mixed to form a transparent solution (DES), and a non-covalent cross-linking agent, aluminum nitrate nonahydrate (Al(NO3)3·9H2O), was added and fully dissolved by ultrasonication; Subsequently, amino-terminated hyperbranched aramid (AF-AP) and photoinitiator (I2959) were added and mixed evenly; finally, the resulting mixture was transferred to a mold, and a polymerizable low-melting gel conductive elastomer based on supramolecular cross-linking, namely, PDES / Al / AF-AP conductive elastomer, was prepared through a photocuring cross-linking reaction.

2. The preparation method according to claim 1, characterized in that Here are the steps: Step 1: mixing choline chloride (ChCl) and acrylic acid (AA) in a certain molar ratio to form a mixture; heating and stirring the mixture to obtain a solution A that can remain clear and transparent at room temperature; Step 2: weigh an appropriate amount of aluminum nitrate nonahydrate (Al(NO3)3·9H2O) and mix it with solution A, and perform ultrasonic treatment to form solution B; Step 3: Weigh an appropriate amount of amino-terminated hyperbranched aramid (AF-AP) and mix with solution B, stir and disperse evenly, then add the photoinitiator (I2959), and stir again to form a precursor solution C; Step 4: Pour the obtained precursor solution C into a polytetrafluoroethylene mold and place it under ultraviolet light for curing, thereby preparing a PDES / Al / AF-AP conductive elastomer.

3. The preparation method according to claim 2, characterized in that: The molar ratio of choline chloride (ChCl) to acrylic acid (AA) is 1:1.5-2.5, the mass ratio of solution A to aluminum nitrate nonahydrate (Al(NO3)3·9H2O) is 100-200:1, the mass ratio of solution A to amino-terminated hyperbranched aramid (AF-AP) is 100:0.1-1, and the mass ratio of solution A to photoinitiator (I2959) is 500-1000:

1.

4. The preparation method according to claim 2, characterized in that: In step 1, the mixture is heated and stirred at 80-100° C. for 1-5 h.

5. The preparation method according to claim 2, characterized in that: In step 3, after adding amino-terminated hyperbranched aramid (AF-AP) and initiator, stir for 10 to 30 minutes respectively to achieve uniform mixing, the stirring temperature is 25 to 30° C., and the stirring speed is 300 to 400 rpm.

6. The preparation method according to claim 2, characterized in that: In step 4, the photocuring cross-linking reaction is cured under ultraviolet light with a wavelength of 365 nm for 60 to 600 seconds, and the reaction temperature is 25 to 30°C.

7. A polymerizable eutectic gel conductive elastomer based on supramolecular cross-linking prepared by the method according to any one of claims 1 to 6.

8. Application of the polymerizable eutectic gel conductive elastomer based on supramolecular cross-linking as claimed in claim 7 in a wearable sensor for detecting human body movement.

Citation Information

Cited By

  • MXene doping-based polycarbonate conductive elastomer as well as preparation method and application thereof

    CN120988448A

  • Polycarbonate-based conductive elastomer based on mxene doping and preparation method and application thereof

    CN120988448B