Plant fiber-based PP recycled household appliance shell material and preparation method thereof

By adding modifiers and magnesium-based organic frame structure to the PP recycled material, the problems of low mechanical strength and electrostatic absorption of dust in PP recycled materials are solved, and the preparation of home appliance housing materials with high mechanical properties and conductivity is achieved.

CN119019804APending Publication Date: 2024-11-26DONGGUAN YUJIE IND INVESTMENT CO LTD

Patent Information

Application Number
CN202411171312.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing PP recycled materials have low mechanical strength and are prone to static electricity, resulting in the problem of adsorbing dust during the use of home appliances.

Method used

The preparation method of plant fiber-based PP cycle regeneration household appliance shell material is adopted, and the modifier is prepared by reacting raw materials such as maleic anhydride and p-nitroaniline, and blending it with PP recycled material, diisopropyl peroxide and other substances. Form a modified polyethylene liquid, and add a modified filler to form a magnesium-based organic frame to enhance the mechanical properties of the material and avoid static electricity.

Benefits of technology

It improves the mechanical properties and conductivity of the home appliance housing materials, avoids the problem of electrostatic absorption of dust, and significantly improves the use effect of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a plant fiber-based PP recycled household appliance shell material and a preparation method thereof.The preparation method comprises the steps that a PP recycled material, a modifier and xylene serve as raw materials and react, modified polyethylene liquid is prepared, aniline, concentrated hydrochloric acid and deionized water are mixed and stirred, the modified polyethylene liquid and modified filler are added, a reaction is conducted, drying and extrusion granulation are conducted, and the plant fiber-based PP recycled household appliance shell material is obtained. A polyaniline structure is formed between a modified polypropylene molecular chain and a modified filler, meanwhile, a magnesium-based organic framework on the surface of the modified filler is a two-dimensional pi conjugated system, a conductive path can be formed between the modified polypropylene molecular chain and the modified filler, and then the shell material is prevented from generating static electricity; the interface acting force of modified polypropylene molecules and the modified filler is improved through connection of polyaniline, the chain-shaped polypropylene molecules are converted into branched structures, the modified filler is coated, cellulose serves as a core of the modified filler, a magnesium organic framework serves as a shell of the modified filler, and then the mechanical performance of the shell material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PP recycled material preparation, and in particular to a plant fiber-based PP recycled household appliance shell material and a preparation method thereof. Background Art

[0002] As the production and sales volume of the home appliance industry increases year by year, people's pursuit of quality of life is also getting higher and higher. However, in the process of pursuing high-performance home appliance products, the problem of handling home appliance waste has become increasingly prominent. Among them, a large number of shell materials are difficult to recycle, which not only occupies a large amount of land resources, but also causes serious pollution to the environment. To solve the above problems, at present, the existing PP recycled home appliance shell materials are mainly divided into the following types: 1. By recycling the shells of discarded home appliances, they are directly used to produce new home appliance shell materials after cleaning, crushing, drying, puffing and other process treatments. 2. On the basis of pure PP recycled materials, a certain proportion of modifiers, enhancers, etc. are added to improve the material performance and realize recycling at the same time. 3. The waste PP material is subjected to high-temperature cracking to obtain low-molecular-weight PP monomers, and then polymerized to synthesize polymers to obtain recycled PP materials. However, the existing PP recycled materials have low mechanical strength, and during the use of home appliances, static electricity will be generated on the surface of the shell, thereby adsorbing dust. Summary of the invention

[0003] The purpose of the present invention is to provide a plant fiber-based PP recycled household appliance housing material and a preparation method thereof, so as to solve the problem that the current PP recycled material has low mechanical strength and is prone to static electricity.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for preparing a plant fiber-based PP recycled household appliance housing material, specifically comprising the following steps:

[0006] Step A1: maleic anhydride and acetone are mixed uniformly, and p-nitroaniline is added under stirring at a speed of 120-150 r / min and a temperature of 0°C, and the temperature is raised to 8-10°C, and the reaction is carried out for 10-15 minutes, and the temperature is raised to 55-60°C, and the reaction is carried out for 30-40 minutes, and triethylamine, acetic anhydride and nickel acetate are added, and the reaction is carried out for 2-3 hours to obtain intermediate 1, and intermediate 1, tin powder and concentrated hydrochloric acid are mixed uniformly, and the reaction is carried out at a speed of 120-150 r / min and a temperature of 90-95°C for 1-1.5 hours, and ammonia water is added to a pH value of 8 to obtain a modifier;

[0007] Step A2: PP recycled material, modifier and xylene are mixed evenly, nitrogen is introduced for protection, diisopropylbenzene peroxide is added under the condition of a rotation speed of 150-200r / min and a temperature of 130-135°C, and the mixture is stirred for 3-5h to obtain a modified polyethylene liquid, aniline, concentrated hydrochloric acid and deionized water are mixed evenly, modified polyethylene liquid and modified filler are added under the condition of a rotation speed of 120-150r / min and a temperature of 3-5°C, and the mixture is stirred for 10-15min, ammonium persulfate is added, the mixture is reacted for 6-8h, the mixture is dried and extruded and granulated under the condition of a head temperature of 190°C, a temperature of 200°C in the first zone, a temperature of 210°C in the second zone, a temperature of 220°C in the third zone, a temperature of 210°C in the fourth zone and a temperature of 200°C in the fifth zone to obtain a home appliance housing material.

[0008] Furthermore, the dosage ratio of maleic anhydride, p-nitroaniline, triethylamine, acetic anhydride and nickel acetate described in step A1 is 50mmo l:50mmo l:5mL:12mL:3.5g, the dosage ratio of intermediate 1, tin powder and concentrated hydrochloric acid is 6mmo l:2g:5mL, and the mass fraction of concentrated hydrochloric acid is 36%.

[0009] Furthermore, the amount ratio of the PP recycled material, modifier, xylene and diisopropylbenzene peroxide described in step A2 is 15g:1g:150mL:0.12g, and the amount ratio of aniline, concentrated hydrochloric acid, deionized water, modified polyethylene liquid, modified filler and ammonium persulfate is 1g:16mL:100mL:150mL:1-3g:1-1.5g.

[0010] Further, the modified filler is prepared by the following steps:

[0011] Step B1: cellulose, sodium hydroxide and anhydrous ethanol are mixed evenly, reacted for 1-1.5 hours at a speed of 120-150 r / min and a temperature of 25-30° C., chloroacetic acid is added, the temperature is raised to 75-80° C., and the reaction is carried out for 2-3 hours to obtain carboxymethyl cellulose; carboxymethyl cellulose, 4-aminophenylboronic acid pinacol ester, aniline, dicyclohexylcarbodiimide and DMF are mixed, and reacted for 3-5 hours at a speed of 200-300 r / min and a temperature of 40-50° C. to obtain pretreated cellulose;

[0012] Step B2: pretreated cellulose, sodium periodate, tetrahydrofuran and deionized water are mixed uniformly, stirred and hydrochloric acid solution is added at a speed of 120-150 r / min and a temperature of 25-30° C., and reacted for 3-4 hours to obtain modified cellulose; modified cellulose, hexahydroxytriphenylene, 5A molecular sieve and DMF are mixed uniformly, and reacted at a speed of 150-200 r / min and a temperature of 70-80° C. for 10-15 hours to obtain a precursor;

[0013] Step B3: The precursor, hexahydroxytriphenylene, magnesium chloride hexahydrate and deionized water are mixed evenly, stirred and ammonia water is added at a speed of 200-300 r / min and a temperature of 85-90°C, and the reaction is carried out for 45-50 hours. The supernatant is removed by centrifugation, and the substrate is washed with acetone and dried to obtain a modified filler.

[0014] Furthermore, the amount ratio of cellulose, sodium hydroxide, anhydrous ethanol and chloroacetic acid in step B1 is 5g:6g:150mL:6g, and the molar ratio of carboxyl group on carboxymethyl cellulose, 4-aminophenylboronic acid pinacol ester, aniline and dicyclohexylcarbodiimide is 3:1:2:3.1.

[0015] Furthermore, the dosage ratio of the pretreated cellulose, sodium periodate, tetrahydrofuran, deionized water and hydrochloric acid solution in step B2 is 3g:15mmo l:40mL:10mL:2mL, the mass fraction of the hydrochloric acid solution is 10%, and the dosage ratio of the boric acid group on the modified cellulose, hexahydroxytriphenylene and 5A molecular sieve is 15mmo l:15mmo l:2g.

[0016] Furthermore, the amount ratio of the precursor, magnesium chloride hexahydrate, deionized water and ammonia water described in step B3 is 2g:1.7g:500mL:2mL, and the mass fraction of ammonia water is 25%.

[0017] The beneficial effects of the invention are as follows: the plant fiber-based PP recycled household appliance shell material disclosed by the invention uses PP recycled material, a modifier and xylene as raw materials, stirs and adds diisopropylbenzene peroxide to react, and obtains a modified polyethylene liquid; aniline, concentrated hydrochloric acid and deionized water are mixed and stirred, and the modified polyethylene liquid and the modified filler are added, stirred, and ammonium persulfate is added to react, and dried and extruded into granules to obtain the household appliance shell material; the modifier uses maleic anhydride and p-nitroaniline as raw materials, so that the maleic anhydride is ring-opened and reacts with the amino group on the p-nitroaniline and closes the ring to obtain an intermediate 1; the intermediate 1 is reduced with tin powder so that the nitro group on the intermediate 1 is converted into an amino group to obtain the modifier; the PP recycled material and the modifier are subjected to the action of diisopropylbenzene peroxide so that the double bonds on the modifier are grafted with the PP recycled material molecular chain; the aniline, the modified polyethylene liquid and the modified filler are blended; under the action of concentrated hydrochloric acid, a polyaniline structure is formed between the modified polypropylene molecular chain and the modified filler.

[0018] The modified filler uses cellulose and chloroacetic acid as raw materials, so that the hydroxyl group on the cellulose and the chlorine atom site on the chloroacetic acid are grafted to obtain carboxymethyl cellulose, the carboxymethyl cellulose, 4-aminophenylboronic acid pinacol ester and aniline are subjected to a dehydration reaction in dicyclohexylcarbodiimide, so that the carboxyl group on the carboxymethyl cellulose and the amino group on the 4-aminophenylboronic acid pinacol ester and the amino group on the aniline are dehydrated to obtain pretreated cellulose, the pretreated cellulose is treated with sodium periodate, so that the structure of the phenylboronic acid pinacol ester is converted into a phenylboronic acid structure to obtain modified cellulose, the modified cellulose is reacted with hexahydroxytriphenylene, so that the boric acid on the modified cellulose and part of the catechol on the hexahydroxytriphenylene react to obtain a precursor, the precursor, the hexahydroxytriphenylene and magnesium chloride hexahydrate are reacted, so that the catechol on the surface of the precursor and the catechol on the hexahydroxytriphenylene react with magnesium ions to form a magnesium-based organic framework to obtain the modified filler.

[0019] A polyaniline structure is formed between the modified polypropylene molecular chain and the modified filler. At the same time, the magnesium-based organic framework on the surface of the modified filler is a two-dimensional π-conjugated system, which can form a conductive path between the modified polypropylene molecular chain and the modified filler, thereby avoiding the generation of static electricity in the shell material. The interfacial force between the modified polypropylene molecules and the modified filler is improved through the connection of polyaniline, and the chain-like polypropylene molecules are transformed into a branched structure and coated with the modified filler. The modified filler has cellulose as the core and the magnesium organic framework as the shell, thereby improving the mechanical properties of the shell material. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1

[0022] A method for preparing a plant fiber-based PP recycled household appliance housing material, specifically comprising the following steps:

[0023] Step A1: maleic anhydride and acetone are mixed uniformly, and p-nitroaniline is added under stirring at a speed of 120 r / min and a temperature of 0°C, and the temperature is raised to 8°C, and the reaction is carried out for 10 minutes, and the temperature is raised to 55°C, and the reaction is carried out for 30 minutes, and triethylamine, acetic anhydride and nickel acetate are added, and the reaction is carried out for 2 hours to obtain intermediate 1, and intermediate 1, tin powder and concentrated hydrochloric acid are mixed uniformly, and the reaction is carried out at a speed of 120 r / min and a temperature of 90°C for 1 hour, and ammonia water is added to a pH value of 8 to obtain a modifier;

[0024] Step A2: Mix the PP recycled material, the modifier and the xylene evenly, introduce nitrogen protection, stir and add diisopropylbenzene peroxide at a speed of 150 r / min and a temperature of 130°C, react for 3 hours to obtain a modified polyethylene liquid, mix aniline, concentrated hydrochloric acid and deionized water evenly, stir and add the modified polyethylene liquid and the modified filler at a speed of 120 r / min and a temperature of 3°C, stir for 10 minutes, add ammonium persulfate, react for 6 hours, dry and extrude and granulate at a head temperature of 190°C, a zone temperature of 200°C, a zone temperature of 210°C, a zone temperature of 320°C, a zone temperature of 210°C, a zone temperature of 420°C, and a zone temperature of 200°C to obtain a home appliance housing material.

[0025] The amount ratio of maleic anhydride, p-nitroaniline, triethylamine, acetic anhydride and nickel acetate described in step A1 is 50mmol:50mmo l:5mL:12mL:3.5g, the amount ratio of intermediate 1, tin powder and concentrated hydrochloric acid is 6mmo l:2g:5mL, and the mass fraction of concentrated hydrochloric acid is 36%.

[0026] The amount ratio of the PP recycled material, modifier, xylene and diisopropylbenzene peroxide described in step A2 is 15g:1g:150mL:0.12g, the amount ratio of aniline, concentrated hydrochloric acid, deionized water, modified polyethylene liquid, modified filler and ammonium persulfate is 1g:16mL:100mL:150mL:1g:1g, and the PP recycled material is PP20 recycled material.

[0027] The modified filler is prepared by the following steps:

[0028] Step B1: cellulose, sodium hydroxide and anhydrous ethanol are mixed evenly, reacted at a speed of 120 r / min and a temperature of 25° C. for 1 hour, chloroacetic acid is added, the temperature is raised to 75° C., and the reaction is carried out for 2 hours to obtain carboxymethyl cellulose; carboxymethyl cellulose, 4-aminophenylboronic acid pinacol ester, aniline, dicyclohexylcarbodiimide and DMF are mixed, and reacted at a speed of 200 r / min and a temperature of 40° C. for 3 hours to obtain pretreated cellulose;

[0029] Step B2: pretreated cellulose, sodium periodate, tetrahydrofuran and deionized water were mixed evenly, stirred and hydrochloric acid solution was added at a speed of 120 r / min and a temperature of 25°C, and reacted for 3 hours to obtain modified cellulose; modified cellulose, hexahydroxytriphenylene, 5A molecular sieve and DMF were mixed evenly, and reacted at a speed of 150 r / min and a temperature of 70°C for 10 hours to obtain a precursor;

[0030] Step B3: The precursor, hexahydroxytriphenylene, magnesium chloride hexahydrate and deionized water are mixed evenly, stirred and ammonia water is added at a speed of 200 r / min and a temperature of 85°C, and the reaction is carried out for 45 hours. The supernatant is removed by centrifugation, and the substrate is washed with acetone and dried to obtain a modified filler.

[0031] The amount ratio of cellulose, sodium hydroxide, anhydrous ethanol and chloroacetic acid described in step B1 is 5g:6g:150mL:6g, and the molar ratio of carboxyl group on carboxymethyl cellulose, 4-aminophenylboronic acid pinacol ester, aniline and dicyclohexylcarbodiimide is 3:1:2:3.1.

[0032] The amount ratio of the pretreated cellulose, sodium periodate, tetrahydrofuran, deionized water and hydrochloric acid solution described in step B2 is 3g:15mmo l:40mL:10mL:2mL, the mass fraction of the hydrochloric acid solution is 10%, and the amount ratio of the boric acid group on the modified cellulose, hexahydroxytriphenylene and 5A molecular sieve is 15mmo l:15mmo l:2g.

[0033] The amount ratio of the precursor, magnesium chloride hexahydrate, deionized water and ammonia water described in step B3 is 2g:1.7g:500mL:2mL, and the mass fraction of ammonia water is 25%.

[0034] Example 2

[0035] A method for preparing a plant fiber-based PP recycled household appliance housing material, specifically comprising the following steps:

[0036] Step A1: maleic anhydride and acetone are mixed uniformly, and p-nitroaniline is added under stirring at a speed of 120 r / min and a temperature of 0°C, and the temperature is raised to 9°C, and the reaction is carried out for 10 minutes, and the temperature is raised to 58°C, and the reaction is carried out for 35 minutes, and triethylamine, acetic anhydride and nickel acetate are added, and the reaction is carried out for 2.5 hours to obtain intermediate 1, and intermediate 1, tin powder and concentrated hydrochloric acid are mixed uniformly, and the reaction is carried out at a speed of 120 r / min and a temperature of 95°C for 1 hour, and ammonia water is added to a pH value of 8 to obtain a modifier;

[0037] Step A2: Mix the PP recycled material, the modifier and the xylene evenly, introduce nitrogen protection, stir and add diisopropylbenzene peroxide at a speed of 150 r / min and a temperature of 135°C, react for 4 hours to obtain a modified polyethylene liquid, mix aniline, concentrated hydrochloric acid and deionized water evenly, stir and add the modified polyethylene liquid and the modified filler at a speed of 120 r / min and a temperature of 4°C, stir for 10 minutes, add ammonium persulfate, react for 7 hours, dry and extrude and granulate at a head temperature of 190°C, a zone temperature of 200°C, a zone temperature of 210°C, a zone temperature of 320°C, a zone temperature of 210°C, a zone temperature of 420°C, and a zone temperature of 200°C to obtain a home appliance housing material.

[0038] The amount ratio of maleic anhydride, p-nitroaniline, triethylamine, acetic anhydride and nickel acetate described in step A1 is 50mmol:50mmo l:5mL:12mL:3.5g, the amount ratio of intermediate 1, tin powder and concentrated hydrochloric acid is 6mmo l:2g:5mL, and the mass fraction of concentrated hydrochloric acid is 36%.

[0039] The amount ratio of the PP recycled material, modifier, xylene and diisopropylbenzene peroxide described in step A2 is 15g:1g:150mL:0.12g, the amount ratio of aniline, concentrated hydrochloric acid, deionized water, modified polyethylene liquid, modified filler and ammonium persulfate is 1g:16mL:100mL:150mL:2g:1.3g, and the PP recycled material is PP20 recycled material.

[0040] The modified filler is prepared by the following steps:

[0041] Step B1: cellulose, sodium hydroxide and anhydrous ethanol are mixed evenly, reacted at a speed of 120-150 r / min and a temperature of 28° C. for 1.3 hours, chloroacetic acid is added, the temperature is raised to 78° C., and the reaction is carried out for 2.5 hours to obtain carboxymethyl cellulose; carboxymethyl cellulose, 4-aminophenylboronic acid pinacol ester, aniline, dicyclohexylcarbodiimide and DMF are mixed, and reacted at a speed of 200 r / min and a temperature of 45° C. for 4 hours to obtain pretreated cellulose;

[0042] Step B2: pretreated cellulose, sodium periodate, tetrahydrofuran and deionized water were mixed uniformly, stirred and hydrochloric acid solution was added at a speed of 120 r / min and a temperature of 28°C, and the mixture was reacted for 3.5 hours to obtain modified cellulose; modified cellulose, hexahydroxytriphenylene, 5A molecular sieve and DMF were mixed uniformly, and the mixture was reacted at a speed of 150 r / min and a temperature of 75°C for 13 hours to obtain a precursor;

[0043] Step B3: The precursor, hexahydroxytriphenylene, magnesium chloride hexahydrate and deionized water are mixed evenly, stirred and ammonia water is added at a speed of 200 r / min and a temperature of 90°C, and the reaction is carried out for 45 hours. The supernatant is removed by centrifugation, and the substrate is washed with acetone and dried to obtain a modified filler.

[0044] The amount ratio of cellulose, sodium hydroxide, anhydrous ethanol and chloroacetic acid described in step B1 is 5g:6g:150mL:6g, and the molar ratio of carboxyl group on carboxymethyl cellulose, 4-aminophenylboronic acid pinacol ester, aniline and dicyclohexylcarbodiimide is 3:1:2:3.1.

[0045] The amount ratio of the pretreated cellulose, sodium periodate, tetrahydrofuran, deionized water and hydrochloric acid solution described in step B2 is 3g:15mmo l:40mL:10mL:2mL, the mass fraction of the hydrochloric acid solution is 10%, and the amount ratio of the boric acid group on the modified cellulose, hexahydroxytriphenylene and 5A molecular sieve is 15mmo l:15mmo l:2g.

[0046] The amount ratio of the precursor, magnesium chloride hexahydrate, deionized water and ammonia water described in step B3 is 2g:1.7g:500mL:2mL, and the mass fraction of ammonia water is 25%.

[0047] Example 3

[0048] A method for preparing a plant fiber-based PP recycled household appliance housing material, specifically comprising the following steps:

[0049] Step A1: maleic anhydride and acetone are mixed uniformly, and p-nitroaniline is added under stirring at a speed of 150 r / min and a temperature of 0°C, and the temperature is raised to 10°C, and the reaction is carried out for 15 minutes, and the temperature is raised to 60°C, and the reaction is carried out for 40 minutes, and triethylamine, acetic anhydride and nickel acetate are added, and the reaction is carried out for 3 hours to obtain intermediate 1, and intermediate 1, tin powder and concentrated hydrochloric acid are mixed uniformly, and the reaction is carried out at a speed of 150 r / min and a temperature of 95°C for 1.5 hours, and ammonia water is added to a pH value of 8 to obtain a modifier;

[0050] Step A2: Mix the PP recycled material, the modifier and the xylene evenly, introduce nitrogen protection, stir and add diisopropylbenzene peroxide at a speed of 200 r / min and a temperature of 135°C, react for 5 hours to obtain a modified polyethylene liquid, mix aniline, concentrated hydrochloric acid and deionized water evenly, stir and add the modified polyethylene liquid and the modified filler at a speed of 150 r / min and a temperature of 5°C, stir for 15 minutes, add ammonium persulfate, react for 8 hours, dry and extrude and granulate at a head temperature of 190°C, a zone temperature of 200°C, a zone temperature of 210°C, a zone temperature of 320°C, a zone temperature of 210°C, a zone temperature of 420°C, and a zone temperature of 200°C to obtain a home appliance housing material.

[0051] The amount ratio of maleic anhydride, p-nitroaniline, triethylamine, acetic anhydride and nickel acetate described in step A1 is 50mmol:50mmo l:5mL:12mL:3.5g, the amount ratio of intermediate 1, tin powder and concentrated hydrochloric acid is 6mmo l:2g:5mL, and the mass fraction of concentrated hydrochloric acid is 36%.

[0052] The amount ratio of the PP recycled material, modifier, xylene and diisopropylbenzene peroxide described in step A2 is 15g:1g:150mL:0.12g, the amount ratio of aniline, concentrated hydrochloric acid, deionized water, modified polyethylene liquid, modified filler and ammonium persulfate is 1g:16mL:100mL:150mL:1-3g:1-1.5g, and the PP recycled material is PP20 recycled material.

[0053] The modified filler is prepared by the following steps:

[0054] Step B1: cellulose, sodium hydroxide and anhydrous ethanol are mixed evenly, reacted at a speed of 150 r / min and a temperature of 30° C. for 1.5 hours, chloroacetic acid is added, the temperature is raised to 80° C., and the reaction is carried out for 3 hours to obtain carboxymethyl cellulose; carboxymethyl cellulose, 4-aminophenylboronic acid pinacol ester, aniline, dicyclohexylcarbodiimide and DMF are mixed, and reacted at a speed of 300 r / min and a temperature of 50° C. for 5 hours to obtain pretreated cellulose;

[0055] Step B2: pretreated cellulose, sodium periodate, tetrahydrofuran and deionized water were mixed uniformly, stirred and hydrochloric acid solution was added at a speed of 150 r / min and a temperature of 30°C, and reacted for 4 hours to obtain modified cellulose; modified cellulose, hexahydroxytriphenylene, 5A molecular sieve and DMF were mixed uniformly, and reacted at a speed of 200 r / min and a temperature of 80°C for 15 hours to obtain a precursor;

[0056] Step B3: The precursor, hexahydroxytriphenylene, magnesium chloride hexahydrate and deionized water were mixed evenly, stirred and ammonia water was added at a speed of 300 r / min and a temperature of 90°C, and the reaction was carried out for 50 hours. The supernatant was removed by centrifugation, and the substrate was washed with acetone and dried to obtain a modified filler.

[0057] The amount ratio of cellulose, sodium hydroxide, anhydrous ethanol and chloroacetic acid described in step B1 is 5g:6g:150mL:6g, and the molar ratio of carboxyl group on carboxymethyl cellulose, 4-aminophenylboronic acid pinacol ester, aniline and dicyclohexylcarbodiimide is 3:1:2:3.1.

[0058] The amount ratio of the pretreated cellulose, sodium periodate, tetrahydrofuran, deionized water and hydrochloric acid solution described in step B2 is 3g:15mmo l:40mL:10mL:2mL, the mass fraction of the hydrochloric acid solution is 10%, and the amount ratio of the boric acid group on the modified cellulose, hexahydroxytriphenylene and 5A molecular sieve is 15mmo l:15mmo l:2g.

[0059] The amount ratio of the precursor, magnesium chloride hexahydrate, deionized water and ammonia water described in step B3 is 2g:1.7g:500mL:2mL, and the mass fraction of ammonia water is 25%.

[0060] Comparative Example 1

[0061] Compared with Example 1, no modifier was added in this comparative example, and the remaining steps were the same.

[0062] Comparative Example 2

[0063] Compared with Example 1, no modified filler was added in this comparative example, and the remaining steps were the same.

[0064] Comparative Example 3

[0065] Compared with Example 1, this comparative example uses graphene instead of the modified filler, and the remaining steps are the same.

[0066] Comparative Example 4

[0067] Compared with Example 1, this comparative example uses cellulose instead of the modified filler, and the other steps are the same.

[0068] Comparative Example 5

[0069] Compared with Example 1, this comparative example uses carboxymethyl cellulose, 4-aminophenylboronic acid pinacol ester, dicyclohexylcarbodiimide and DMF to mix, and reacts at a speed of 200 r / min and a temperature of 40° C. for 3 hours. The obtained product replaces the pretreated cellulose, and the remaining steps are the same.

[0070] Comparative Example 6

[0071] Compared with Example 1, this comparative example uses carboxymethyl cellulose, aniline, dicyclohexylcarbodiimide and DMF to mix, and reacts for 3 hours at a speed of 200 r / min and a temperature of 40° C. The obtained product replaces the pretreated cellulose, and the remaining steps are the same.

[0072] The shell materials prepared in Examples 1-3 and Comparative Examples 1-6 supported samples of 12 cm × 4 cm × 0.4 cm. The tensile strength was tested at a stretching speed of 50 mm / min in accordance with the standard of GB / T1040.1-2018. The impact strength was tested in accordance with the standard of GB / T1043.2-2018. The surface resistance was tested in accordance with the standard of B / T1410-2006. The test results are shown in the following table.

[0073] Tensile strength MPa <![CDATA[Impact strength kJ / m 2 > Surface resistivity Ω / sq Example 1 68.9 56.9 <![CDATA[1.01×10 7 ]]> Example 2 71.6 58.6 <![CDATA[1.01×10 7 ]]> Example 3 73.1 59.3 <![CDATA[1.01×10 7 ]]> Comparative Example 1 57.3 50.5 <![CDATA[8.34×10 8 ]]> Comparative Example 2 41.7 28.4 <![CDATA[5.02×10 8 ]]> Comparative Example 3 57.1 34.3 <![CDATA[2.28×10 8 ]]> Comparative Example 4 55.4 32.5 <![CDATA[1.12×10 9 ]]> Comparative Example 5 65.3 54.8 <![CDATA[9.37×10 7 ]]> Comparative Example 6 62.7 53.5 <![CDATA[8.99×10 7 ]]>

[0074] It can be seen from the above table that the present application has good mechanical properties and electrical conductivity.

[0075] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a plant fiber-based PP recycled household appliance housing material, characterized in that: The specific steps include: Step A1: maleic anhydride and acetone are mixed and stirred, and p-nitroaniline is added, the temperature is raised for reaction, triethylamine, acetic anhydride and nickel acetate are added, and the reaction is continued to obtain intermediate 1, intermediate 1, tin powder and concentrated hydrochloric acid are mixed for reaction, and ammonia water is added to obtain a modifier; Step A2: Evenly mix the PP recycled material, the modifier and the xylene, introduce nitrogen protection, stir and add diisopropylbenzene peroxide to react to obtain a modified polyethylene liquid, mix and stir aniline, concentrated hydrochloric acid and deionized water, add the modified polyethylene liquid and the modified filler, stir, add ammonium persulfate, react, dry and extrude into granules to obtain a home appliance housing material.

2. The method for preparing a plant fiber-based PP recycled household appliance housing material according to claim 1, characterized in that: The amount ratio of maleic anhydride, p-nitroaniline, triethylamine, acetic anhydride and nickel acetate described in step A1 is 50mmol:50mmol:5mL:12mL:3.5g, and the amount ratio of intermediate 1, tin powder and concentrated hydrochloric acid is 6mmol:2g:5mL.

3. The method for preparing a plant fiber-based PP recycled household appliance housing material according to claim 1, characterized in that: The amount ratio of the PP recycled material, modifier, xylene and diisopropylbenzene peroxide described in step A2 is 15g:1g:150mL:0.12g, and the amount ratio of aniline, concentrated hydrochloric acid, deionized water, modified polyethylene liquid, modified filler and ammonium persulfate is 1g:16mL:100mL:150mL:1-3g:1-1.5g.

4. The method for preparing a plant fiber-based PP recycled household appliance housing material according to claim 1, characterized in that: The modified filler is prepared by the following steps: Step B1: After cellulose, sodium hydroxide and anhydrous ethanol are mixed for reaction, chloroacetic acid is added, and the temperature is raised to react to obtain carboxymethyl cellulose; carboxymethyl cellulose, 4-aminophenylboronic acid pinacol ester, aniline, dicyclohexylcarbodiimide and DMF are mixed for reaction to obtain pretreated cellulose; Step B2: mixing and stirring modified cellulose, sodium periodate, tetrahydrofuran and deionized water, and adding hydrochloric acid solution to react to obtain modified cellulose; mixing and reacting modified cellulose, hexahydroxytriphenylene, 5A molecular sieve and DMF to obtain a precursor; Step B3: The precursor, hexahydroxytriphenylene, magnesium chloride hexahydrate and deionized water are mixed and stirred, and ammonia water is added to react. The supernatant is removed by centrifugation, and the substrate is washed with acetone and dried to obtain a modified filler.

5. The method for preparing a plant fiber-based PP recycled household appliance housing material according to claim 4, characterized in that: The amount ratio of cellulose, sodium hydroxide, anhydrous ethanol and chloroacetic acid described in step B1 is 5g:6g:150mL:6g, and the molar ratio of carboxyl group on carboxymethyl cellulose, 4-aminophenylboronic acid pinacol ester, aniline and dicyclohexylcarbodiimide is 3:1:2:3.

1.

6. The method for preparing a plant fiber-based PP recycled household appliance housing material according to claim 4, characterized in that: The amount ratio of the pretreated cellulose, sodium periodate, tetrahydrofuran, deionized water and hydrochloric acid solution described in step B2 is 3g:15mmol:40mL:10mL:2mL, the mass fraction of the hydrochloric acid solution is 10%, and the amount ratio of the boric acid group on the modified cellulose, hexahydroxytriphenylene and 5A molecular sieve is 15mmol:15mmol:2g.

7. The method for preparing a plant fiber-based PP recycled household appliance housing material according to claim 4, characterized in that: The amount ratio of the precursor, magnesium chloride hexahydrate, deionized water and ammonia water described in step B3 is 2g:1.7g:500mL:2mL.

8. A plant fiber-based PP recycled household appliance housing material, characterized by: Prepared according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Composite diaphragm for lithium battery and preparation method of composite diaphragm

    CN115275520A

  • MOF / cellulose hydrogel as well as preparation method and application thereof

    CN116751374A

  • Magnetic covalent organic framework aerogel for efficiently recovering lithium ions in water

    CN117899767A

Cited By

  • Carbon sequestration type concrete internal curing material based on NaX molecular sieve and preparation method of carbon sequestration type concrete internal curing material

    CN119912192A

  • Environment-friendly gutta-percha modified high-strength material and preparation method thereof

    CN122609032A