Modified glass fiber reinforced epoxy resin composite material and preparation method thereof

Through plasma modification and coupling agent treatment, the interface combination between glass fiber and epoxy resin is improved, and combined with hollow glass microbead enhancement, the problem of insufficient toughness and high temperature resistance of epoxy resin materials is solved, and the composite material is significantly improved Mechanical and insulation properties, suitable for high-end applications.

CN119019813APending Publication Date: 2024-11-26HAINAN POWER GRID CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411043803.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The lack of toughness, impact strength and high temperature resistance of epoxy resin materials limits its application in high-end fields, especially the poor interface bonding performance between glass fiber and epoxy resin, resulting in poor mechanical properties of composite materials.

Method used

Plasma modification and coupling agent treatment are used to increase the number of active groups on the surface of glass fibers, combined with hollow glass microbead reinforcement material, soak the modified glass fibers through plasma surface treatment and coupling agent solution to form covalent bonds and rings The combination of oxygen resin improves interface performance and forms a modified glass fiber reinforced epoxy resin composite material through hot press curing and secondary heating.

Benefits of technology

It significantly improves the breakdown strength and mechanical properties of glass fiber/epoxy resin composites, enhances the structural stability and insulation properties of the material, reduces the weight of the material, improves the interface performance, and is suitable for high-end applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019813A_ABST
    Figure CN119019813A_ABST
Patent Text Reader

Abstract

The invention discloses a modified glass fiber reinforced epoxy resin composite material and a preparation method thereof. According to the method, active groups are introduced to the surfaces of the glass fibers through surface treatment of a silane coupling agent, then the number of the active groups is further increased by combining plasma surface treatment, and more binding sites are provided, so that the interface binding capacity of the glass fibers in a fiber reinforced material and a matrix material epoxy resin is favorably realized; the coupling agent greatly weakens the etching damage of plasma to the surface of the glass fiber, and is more favorable for improving the mechanical property of the material. The particle reinforced material hollow glass beads are also introduced and are uniformly mixed with the matrix material after being treated by the coupling agent, so that the interface bonding strength is improved, the structural stability of the matrix material is maintained, the mechanical property of the matrix material is improved, and the shock-absorbing effect and the insulating property are enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of epoxy resin preparation, and specifically relates to a modified glass fiber reinforced epoxy resin composite material and a preparation method thereof. Background Art

[0002] As an important branch of materials, polymer materials are widely used in all walks of life and have a profound impact on all aspects of people's production and life. Epoxy resin, as an important polymer material, is a thermosetting resin with good comprehensive performance. It has good mechanical properties, bonding properties, good chemical stability, electrical insulation, easy molding and processing, and is widely used in various fields such as automobiles, power electronics, and aerospace. Fiber-reinforced resin molded products can be manufactured by molding fiber-reinforced composite materials using molding methods such as filament winding, compression molding, hand lay-up, pultrusion, and resin transfer molding (RTM). However, epoxy resin also has some disadvantages, such as poor toughness and low impact strength of the cured material, and poor high temperature resistance of the material, which cannot meet the requirements of long-term use at high temperatures. These have greatly restricted the application of epoxy resin in some high-end fields. Moreover, with the continuous development and progress of related industries, the performance requirements for epoxy resin are getting higher and higher. These shortcomings of epoxy resin have gradually restricted its application in high-end fields, limiting the development of epoxy resin materials. How to improve the toughness, impact strength, high temperature resistance, etc. of existing epoxy resin has become the focus of research. Usually, the fiber composite method can effectively achieve the above goals.

[0003] However, composite materials are composed of two or more material components with different chemical and physical properties, combined in a certain form, proportion, and distribution, and there are obvious interfaces between the components. For glass fiber reinforced resin-based composite materials, the interfacial force depends largely on the fiber surface structure, such as surface roughness, pore structure, and active groups, and is also affected by the chemical structure of the matrix. For composite materials, the interface is a bridge between the matrix and the reinforcement, which can transfer force from the matrix to the reinforcement. If the interface area of ​​the composite material is not well bonded, the composite material is prone to interface debonding and cracking, which leads to the destruction of the composite material and the mechanical properties of the reinforced material cannot be brought into play. In addition, the interface can also effectively slow down the propagation of cracks. If the interface performance is poor, it is easy to cause the composite material to be delaminated and damaged. It can be said that the quality of the interface performance directly determines the performance of the entire product, and the surface of the glass fiber is usually smooth and has no active groups, resulting in weak interfacial bonding with the epoxy resin, making it difficult to exert the efficient reinforcement and toughening of the glass fiber. Therefore, how to improve the bonding performance of glass fiber and epoxy resin has become the key to preparing glass fiber reinforced epoxy resin with excellent performance. Surface modification methods can effectively increase the active groups on the surface, thereby improving the surface roughness of the glass fiber material, enhancing the interface properties of the composite material, and achieving the purpose of improving the overall performance of the composite material.

[0004] At present, the surface modification methods for materials mainly include physical modification and chemical modification. Chemical methods mainly include chemical etching, chemical surface grafting, etc. Studies have shown that the surface roughness, interfacial shear strength (IFSS) and other properties are significantly improved after chemical treatment. However, chemical treatment may corrode the surface, introduce defects, and reduce its mechanical properties; in addition, chemical treatment requires a large amount of water and chemicals, which is not environmentally friendly. Physical methods include coating the surface of glass fiber materials, plasma modification, irradiating glass fibers with high-energy rays, ultrasonic impregnation, etc.

[0005] In recent years, plasma treatment has been greatly developed as a physical method for surface modification. Plasma modification is to bombard the fiber surface with plasma. On the one hand, it can increase the roughness and wettability of the fiber surface, thereby improving the bonding strength with the polymer matrix; on the other hand, it can generate active free radicals on the fiber surface, and many active groups can be generated by polymerization with monomers. Compared with chemical etching treatment, plasma treatment reduces the problem of reduced mechanical properties caused by surface defects. In addition, it is a dry process and is therefore environmentally friendly. However, process parameters such as the type of gas, plasma treatment time, discharge power, and the composite process of modified glass fiber and epoxy resin have an important influence on the mechanical and electrical properties of the composite material. On the other hand, it is a common practice to use a coupling agent to treat the glass fiber surface, and the coupling agent is used as an intermediate layer between the fiber and the resin to modify the interface. The coupling agent is like a bridge, spanning between the matrix and the fiber reinforcement, and acts by chemical bonds, greatly improving the bonding force and adhesion between the two, thereby significantly improving the mechanical properties of the material. The amount of coupling agent and the treatment time have an important influence on the mechanical and electrical properties of the composite material. At the same time, glass fiber reinforced epoxy resin composites still need to be further improved in terms of material lightweighting. Summary of the invention

[0006] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0007] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0008] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a modified glass fiber reinforced epoxy resin composite material, characterized in that: the modified glass fiber reinforced epoxy resin composite material comprises an epoxy resin composition and a glass fiber material;

[0009] The epoxy resin composition comprises an epoxy resin having at least two oxirane groups in the molecule, an amine curing agent modified by aliphatic amine and a particle reinforcement material;

[0010] The mass ratio of the epoxy resin, the curing agent and the particle reinforcement material is 100:15-35:0.2-10;

[0011] The glass fiber has surface functional groups capable of forming covalent bonds with epoxy resin; the glass fiber accounts for 20-50% of the total mass of the composite material.

[0012] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a modified glass fiber reinforced epoxy resin composite material, characterized in that: comprising:

[0013] Pre-treatment of glass fiber and particle reinforcement materials;

[0014] The pretreated glass fiber and particle reinforcement material are respectively placed in a coupling agent solution and soaked at 25-50° C. for 3-12 hours, and fixed on a substrate after drying, and the surfaces of the glass fiber and particle reinforcement material are subjected to plasma modification treatment to prepare a modified glass fiber composite material for use;

[0015] Mix the epoxy resin, curing agent and particle reinforcement material, stir evenly and use them as the base material for later use;

[0016] Apply a layer of base material on the inner mold, then lay a layer of modified glass fiber material, and repeat the coating of base material and modified glass fiber material several times;

[0017] The outer mold and the inner mold are closed, hot pressing and curing are performed, and secondary heating and curing are performed after demoulding to obtain a modified glass fiber reinforced epoxy resin composite material.

[0018] As a preferred embodiment of the preparation method of the present invention, the pretreatment includes acetone immersion, deionized water washing and drying, wherein the acetone immersion time is 12 to 24 hours.

[0019] As a preferred embodiment of the preparation method of the present invention, the drying temperature is 50-70° C. and the drying time is 12-24 hours.

[0020] As a preferred solution of the preparation method of the present invention, the coupling agent solution comprises anhydrous ethanol and a coupling agent, and the concentration of the coupling agent is 10-40%.

[0021] As a preferred embodiment of the preparation method of the present invention, the stirring is uniform, wherein the stirring speed is 1000-2000 rpm and the stirring time is 3-10 min.

[0022] As a preferred embodiment of the preparation method of the present invention, the particle reinforcement material is hollow glass microspheres, and the particle size of the hollow glass microspheres is 10 to 80 μm.

[0023] As a preferred embodiment of the preparation method described in the present invention, the parameters of the plasma modification treatment are: using air or oxygen, gas pressure 0-100Pa, high voltage output voltage 3-7kV, frequency 50±1kHz, discharge power 0-100WW, moving speed of the plasma brush 1mm / s, and treatment time 600-900s.

[0024] As a preferred embodiment of the preparation method of the present invention, the glass fiber includes but is not limited to glass fiber woven cloth, short glass fiber, and long glass fiber; the number of layers of the modified glass fiber material is one less than the number of layers of the base material, and the upper and lower layers close to the mold are the base material. After each time the base material is laid, the base material is completely soaked in the modified glass fiber material before being stacked again.

[0025] As a preferred embodiment of the preparation method of the present invention, when the number of layers of the modified glass fiber material is not less than 2, the modified glass fiber material is required to maintain warp consistency during laying.

[0026] Beneficial effects of the present invention:

[0027] (1) The present invention provides a preparation method for improving the performance of glass fiber / epoxy resin composite materials. The method introduces a certain number of active groups into the glass fiber by varying the concentration, treatment time, and treatment temperature of the coupling agent, and then uses plasma surface treatment to add active groups to the surfaces of the glass fiber and hollow glass microspheres where the coupling agent is not attached and to the coupling agent on the surface, thereby providing more binding sites, thereby facilitating the interfacial bonding ability of the fiber-reinforced material glass fiber, the hollow glass microspheres, and the matrix material epoxy resin, and improving the performance of the glass fiber / epoxy resin composite material, such as the breakdown strength. In addition, the coupling agent treatment first helps to reduce the defects on the glass fiber surface caused by the plasma treatment, thereby being more conducive to improving the mechanical properties.

[0028] (2) The present invention also introduces hollow glass microspheres to reinforce the material, uses a coupling agent to increase the interaction between the hollow glass microspheres and the epoxy resin, and mixes them evenly with the matrix material to reduce the weight of the material and improve the structural stability, mechanical properties, shock absorption effect and insulation performance of the matrix material.

[0029] (3) The method disclosed in the present invention is based on the actual production process of glass fiber-hollow glass microsphere-resin composite materials, and is improved from the perspectives of improving the interface and properties of the composite materials and reducing the weight of the materials. It is simple to implement and easy to operate, and has strong industrial applicability. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0031] Figure 1 This is a process flow chart of the modified glass fiber reinforced epoxy resin composite material prepared in Example 1;

[0032] Figure 2 is a SEM image of the modified glass fiber reinforced epoxy resin composite material obtained in Example 1;

[0033] Figure 3 is a SEM image of the modified glass fiber reinforced epoxy resin composite material obtained in Example 2;

[0034] Figure 4 is a SEM image of the modified glass fiber reinforced epoxy resin composite material obtained in Example 3;

[0035] Figure 5 is a SEM image of the modified glass fiber reinforced epoxy resin composite material obtained in Comparative Example 1;

[0036] Figure 6 is a SEM image of the modified glass fiber reinforced epoxy resin composite material obtained in Comparative Example 2;

[0037] Figure 7 This is a graph showing the tensile strength results of the glass fiber reinforced epoxy resin composite materials obtained in Example 3 and Comparative Examples 3 to 6. DETAILED DESCRIPTION

[0038] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0039] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0040] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0041] Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commercially available.

[0042] Example 1

[0043] like Figure 1 As shown, a method for preparing a modified glass fiber reinforced epoxy resin composite material is provided, and the obtained material is applied to insulating ladders and insulating pull rods. The details are as follows:

[0044] First, 0.3 mm glass fiber woven cloth and hollow glass microbeads were immersed in acetone for 24 hours, taken out, placed in a vacuum drying oven at 60° C. for 12 hours, and dried for later use.

[0045] The pretreated glass fibers and glass microbeads were immersed in 25% KH550 coupling agent / anhydrous ethanol solution for 8 hours at a temperature of 40°C.

[0046] The glass fiber and hollow glass microbeads were taken out, dried and fixed on the surface of a clean and flat glass substrate. The size of the glass fiber woven cloth was equal to the size of the glass substrate. The surface of the glass fiber woven cloth was plasma modified in an air environment using a plasma brush as a high-voltage electrode. The treatment conditions were: air was used as the gas source, the high-voltage output voltage was 7kV, the frequency was 50kHz, the discharge power was 80W, the moving speed of the plasma brush was 1mm / s, and the treatment time was 900s.

[0047] In addition, 100 parts by mass of E44, 20 parts by mass of 593 curing agent, and 4 parts by mass of hollow glass microspheres were mixed and stirred evenly in a shearing disperser. The stirring speed of the shearing disperser was 1500 rpm and the stirring time was 10 minutes to obtain a blended system as a matrix material for standby use. The particle size of the hollow glass microspheres was 35 to 45 μm and the true density was 0.30 to 0.34 g / cm 3 .

[0048] Afterwards, prepare materials according to 1 mass part of glass fiber woven cloth and 3 mass parts of matrix material, take the insulating pull rod core shaft as the inner mold, clean it with alcohol, and then apply a layer of thermosetting epoxy resin high temperature resistant mold release agent, and then apply a layer of matrix material (after soaking the glass fiber woven cloth, the woven cloth should not contact the core shaft), and then tightly wrap a layer of the above-treated glass fiber woven cloth, and then apply another layer of matrix material to ensure that the matrix material completely soaks the glass fiber woven cloth and then tightly wrap a layer of treated glass fiber woven cloth. Repeat this operation, apply a total of three layers of matrix material, and wrap two layers of glass fiber woven cloth to obtain a cylindrical structure (the core shaft is not removed at this time), in which the warp directions of the two layers of glass fiber woven cloth remain consistent (the weaving trend of the woven cloth is consistent).

[0049] Finally, an outer mold is put on the outer surface and wrapped tightly, and a pressure of 1 MPa is applied to perform hot pressing and curing at 60°C for 1 hour. After completion, the mold is demolded and the mold is heated to 150°C again for curing for 4 hours to obtain an insulating pull rod made of glass fiber reinforced epoxy resin composite material.

[0050] Example 2

[0051] A method for preparing a modified glass fiber reinforced epoxy resin composite material is as follows:

[0052] First, 0.3 mm glass fiber woven cloth and hollow glass microbeads were immersed in acetone for 16 h, taken out, and then placed in a vacuum drying oven at 60° C. for 12 h for drying and use.

[0053] The pretreated glass fibers and glass microbeads were immersed in a 20% KH550 coupling agent / anhydrous ethanol solution for 6 hours at a temperature of 40°C.

[0054] The glass fiber and hollow glass microbeads were taken out, dried and fixed on the clean and flat surface of the glass substrate. The size of the glass fiber woven cloth was equal to the size of the glass substrate. The surface of the glass fiber woven cloth was plasma modified in an air environment using a plasma brush as a high-voltage electrode. The treatment conditions were: air was used as the gas source, the high-voltage output voltage was 7kV, the frequency was 50kHz, the discharge power was 80W, the moving speed of the plasma brush was 1mm / s, and the treatment time was 720s.

[0055] In addition, 100 parts by mass of E44, 20 parts by mass of 593 curing agent, and 3 parts by mass of hollow glass microspheres were mixed and stirred evenly in a shearing disperser. The stirring speed of the shearing disperser was 1500 rpm and the stirring time was 5 minutes to obtain a blended system as a matrix material for standby use. The particle size of the hollow glass microspheres was 35 to 45 μm and the true density was 0.30 to 0.34 g / cm 3 .

[0056] Afterwards, prepare materials according to 1 mass part of glass fiber woven cloth and 3 mass parts of matrix material, take the insulating pull rod core shaft as the inner mold, clean it with alcohol, and then apply a layer of thermosetting epoxy resin high temperature resistant mold release agent, and then apply a layer of matrix material (after soaking the glass fiber woven cloth, the woven cloth should not contact the core shaft), and then tightly wrap a layer of the above-treated glass fiber woven cloth, and then apply another layer of matrix material to ensure that the matrix material completely soaks the glass fiber woven cloth and then tightly wrap a layer of treated glass fiber woven cloth. Repeat this operation, apply a total of three layers of matrix material, and wrap two layers of glass fiber woven cloth to obtain a cylindrical structure (the core shaft is not removed at this time), in which the warp directions of the two layers of glass fiber woven cloth remain consistent (the weaving trend of the woven cloth is consistent).

[0057] Finally, an outer mold is put on the outer surface and wrapped tightly, and a pressure of 0.8 MPa is applied to perform hot pressing and curing at 60°C for 1 hour. After completion, the mold is demolded and heated to 140°C for curing for 3 hours to obtain an insulating pull rod made of glass fiber reinforced epoxy resin composite material.

[0058] Example 3

[0059] A method for preparing a modified glass fiber reinforced epoxy resin composite material is as follows:

[0060] First, 0.3 mm glass fiber woven cloth and hollow glass microbeads were immersed in acetone for 12 hours respectively, then taken out, and then placed in a vacuum drying oven at 60° C. for 12 hours for drying and set aside.

[0061] The pretreated glass fibers and glass microbeads were immersed in 15% KH550 coupling agent / anhydrous ethanol solution for 6 hours at a temperature of 40°C.

[0062] The glass fiber and hollow glass microbeads were taken out, dried and fixed on the clean and flat surface of the glass substrate. The size of the glass fiber woven cloth was equal to the size of the glass substrate. The surface of the glass fiber woven cloth was plasma modified in an air environment using a plasma brush as a high-voltage electrode. The treatment conditions were: air was used as the gas source, the high-voltage output voltage was 7kV, the frequency was 50kHz, the discharge power was 80W, the moving speed of the plasma brush was 1mm / s, and the treatment time was 600s.

[0063] In addition, 100 parts by mass of E44, 20 parts by mass of 593 curing agent, and 2 parts by mass of hollow glass microspheres were mixed and stirred evenly in a shearing disperser. The stirring speed of the shearing disperser was 1500 rpm and the stirring time was 3 minutes to obtain a blended system as a matrix material for standby use. The particle size of the hollow glass microspheres was 35 to 45 μm and the true density was 0.30 to 0.34 g / cm 3 .

[0064] Afterwards, prepare materials according to 1 mass part of glass fiber woven cloth and 3 mass parts of matrix material, take the insulating pull rod core shaft as the inner mold, clean it with alcohol, and then apply a layer of thermosetting epoxy resin high temperature resistant mold release agent, and then apply a layer of matrix material (after soaking the glass fiber woven cloth, the woven cloth should not contact the core shaft), and then tightly wrap a layer of the above-treated glass fiber woven cloth, and then apply another layer of matrix material to ensure that the matrix material completely soaks the glass fiber woven cloth and then tightly wrap a layer of treated glass fiber woven cloth. Repeat this operation, apply a total of three layers of matrix material, and wrap two layers of glass fiber woven cloth to obtain a cylindrical structure (the core shaft is not removed at this time), in which the warp directions of the two layers of glass fiber woven cloth remain consistent (the weaving trend of the woven cloth is consistent).

[0065] Finally, an outer mold is put on the outer surface and wrapped tightly, and a pressure of 0.5 MPa is applied to perform hot pressing and curing at 60°C for 1 hour. After completion, the mold is demolded and heated to 135°C for curing for 3 hours to obtain an insulating pull rod made of glass fiber reinforced epoxy resin composite material.

[0066] Comparative Example 1

[0067] A method for preparing a modified glass fiber reinforced epoxy resin composite material, which is different from Example 2 in that no plasma treatment is performed.

[0068] Comparative Example 2

[0069] A method for preparing a modified glass fiber reinforced epoxy resin composite material, which is different from Example 2 in that the plasma treatment time is 300 s.

[0070] Comparative Example 3

[0071] A method for preparing a modified fiber reinforced epoxy resin composite material, which is different from Example 3 in that hollow glass microspheres are not added to the matrix material.

[0072] Comparative Example 4

[0073] The difference between this comparative example and Example 3 is that the glass fiber woven cloth is not soaked in KH550, and the remaining steps are the same as those in Example 3.

[0074] Comparative Example 5

[0075] The difference between this comparative example and Example 3 is that the glass fiber woven cloth is not subjected to plasma treatment, and the remaining steps are the same as those in Example 3.

[0076] Comparative Example 6

[0077] The difference between this comparative example and Example 3 is that the glass fiber woven cloth is not treated by soaking in KH550, and hollow glass microspheres are not added to the base material. The remaining steps are the same as those in Example 3.

[0078] Figures 2 to 6 They are SEM images of the composite materials obtained in Example 1, Example 2, Example 3 and Comparative Example 1 and Comparative Example 2 respectively.

[0079] contrast Figures 2 to 6 It can be seen that the etching effect of plasma-treated glass is strongly dependent on the treatment time, and the surface roughness of the glass increases with the increase of treatment time: the fiber surface treated for 15 minutes is uneven and very rough, which indicates that the epoxy resin has a high bonding strength; while the untreated glass surface is clean and smooth, and the adhesion between the glass fiber and the epoxy resin is weak. After 5 minutes of plasma treatment, the glass fiber surface begins to show etching marks, that is, the surface is slightly rough, with slight scratches and bumps, and the bonding between the glass fiber and the epoxy resin is enhanced. From the perspective of surface morphology, the roughness and damage of the fiber surface become more serious with the extension of plasma treatment time, and the coating of the coupling agent can reduce the damage to the glass fiber surface to a certain extent.

[0080] From the comparison of the above SEM images, there is an optimal treatment time for the plasma treatment of glass fibers. In summary, a plasma treatment time of 15 minutes is more successful for the surface modification of glass fibers.

[0081] Figure 7 The mechanical properties of the modified glass fiber reinforced epoxy resin composite materials obtained in Example 3 and Comparative Examples 3 to 6 were compared. The test method was to prepare standard specimens according to GB / T 1040-2006 standard, and the test was carried out at a tensile rate of 20 mm / min. 5 valid data were taken for each group of samples, and the average value and standard deviation were calculated.

[0082] Depend on Figure 7 It can be seen that the mechanical properties of the glass fiber reinforced composite material obtained by the solution of the present invention are significantly better than those of other comparative examples.

[0083] Comparative Example 7

[0084] The difference between this comparative example and Example 3 is that the particle size of the hollow glass microspheres is replaced with 90 μm, and the other steps are the same as Example 3. However, due to its large particle size, it is difficult to exert the particle reinforcement effect, and the large particle size affects the infiltration of the resin and the glass fiber.

[0085] Comparative Example 8

[0086] The difference between this comparative example and Example 3 is that the particle size of the hollow glass microspheres is replaced with 5 μm, and the remaining steps are the same as those of Example 3. Due to its small particle size, it is difficult to exert the particle reinforcement effect.

[0087] Therefore, the particle size of the hollow glass microspheres is selected between 10-80 μm for better promotion effect.

[0088] The present invention combines the advantages of plasma treatment and coupling modification, adjusts the plasma treatment process parameters, combines the coupling agent modification process, improves the bonding mode of glass fiber and epoxy resin matrix material, and obtains a composite material with excellent mechanical properties and electrical properties. In addition, the advantages of low density, high strength, and strong insulation of hollow glass microspheres are also used to achieve lightweight glass fiber reinforced epoxy resin composite materials. On the one hand, in order to avoid excessive defects introduced to the surface of glass fiber and glass microspheres by plasma treatment, resulting in weakened reinforcement; on the other hand, in order to introduce more active groups on the surface of glass fiber and coupling agent, thereby enhancing the interaction between epoxy resin, the glass fiber and hollow glass microspheres are first treated with coupling agent, and then plasma surface treatment is performed.

[0089] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.

Claims

1. A modified glass fiber reinforced epoxy resin composite material, Features: The modified glass fiber reinforced epoxy resin composite material comprises an epoxy resin composition and a glass fiber material; The epoxy resin composition comprises an epoxy resin having at least two oxirane groups in the molecule, an amine curing agent modified by aliphatic amine and a particle reinforcement material; The mass ratio of the epoxy resin, the curing agent and the particle reinforcement material is 100:15-35:0.2-10; The glass fiber has surface functional groups capable of forming covalent bonds with epoxy resin; the glass fiber accounts for 20-50% of the total mass of the composite material.

2. The method for preparing the modified glass fiber reinforced epoxy resin composite material according to claim 1, Features: include, Pre-treatment of glass fiber and particle reinforcement materials; The pretreated glass fiber and particle reinforcement material are placed in a coupling agent solution and soaked at 25-50° C. for 3-12 hours, and fixed on a substrate after drying, and the surfaces of the glass fiber and particle reinforcement material are subjected to plasma modification treatment for standby use; Mix the epoxy resin, curing agent and particle reinforcement material, stir evenly and use them as the base material for later use; Apply a layer of base material on the inner mold, then lay a layer of modified glass fiber material, and repeat the coating of base material and modified glass fiber material several times; The outer mold and the inner mold are closed, hot pressing and curing are performed, and secondary heating and curing are performed after demoulding to obtain a modified glass fiber reinforced epoxy resin composite material.

3. The preparation method according to claim 2, Features: The pretreatment includes acetone immersion, deionized water washing and drying, wherein the acetone immersion time is 12 to 24 hours.

4. The preparation method according to claim 3, Features: The drying temperature is 50-70° C. and the drying time is 12-24 hours.

5. The preparation method according to claim 2, Features: The coupling agent solution comprises anhydrous ethanol and a coupling agent, and the concentration of the coupling agent is 10-40%.

6. The preparation method according to claim 2, Features: The stirring is uniform, wherein the stirring speed is 1000-2000 rpm and the stirring time is 3-10 min.

7. The preparation method according to claim 2, Features: The particle reinforcement material is hollow glass microspheres, and the particle size of the hollow glass microspheres is 10 to 80 μm.

8. The preparation method according to claim 2, Features: The parameters of the plasma modification treatment are: using air or oxygen, gas pressure 0-100Pa, high voltage output voltage 3-7kV, frequency 50±1kHz, discharge power 0-100WW, moving speed of plasma brush 1mm / s, and treatment time 600-900s.

9. The preparation method according to claim 2, Features: The glass fiber includes but is not limited to glass fiber woven cloth, short glass fiber, and long glass fiber; the number of layers of the modified glass fiber material is one less than the number of layers of the base material, and the upper and lower layers close to the mold are the base material. After each time the base material is laid, the base material is completely impregnated with the modified glass fiber composite material before being stacked again.

10. The preparation method according to claim 2, Features: When the number of layers of the modified glass fiber material is not less than 2, the modified glass fiber material is required to maintain warp consistency during laying.

Citation Information

Cited By

  • Method for improving cloth lines after hot pressing of epoxy glass fiber composite material

    CN120842787A

  • Resistive film, broadband wave-absorbing material and preparation method of broadband wave-absorbing material

    CN121528667A

  • A method for modifying the interface plasma cross-linking of the internal insulation of a composite insulator

    CN122968076A