Nucleo-base pair assembled self-repairing material as well as preparation method and application thereof

Through nucleobase pair assembly technology, combined with multiple types of hydrogen bonds, the modified graphene two-dimensional nanosheets form high-density interfacial hydrogen bonds with the matrix material, solving the mechanical strength, tensile and rapid self-repair capabilities of self-repair materials. The contradiction between the two achieves excellent performance in room temperature and low temperature environments.

CN119019837AActive Publication Date: 2024-11-26NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411130233.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

There are contradictions in existing self-healing materials in balancing mechanical strength, tensile properties and rapid room temperature self-healing ability, and it is difficult to meet high mechanical properties, excellent tensile properties and rapid self-healing ability at the same time.

Method used

Through nucleobase pair assembly technology, combining main chain hydrogen bonds, side chain hydrogen bonds and interface hydrogen bonds, high-density nucleobase pair interfacial hydrogen bonds are formed between the modified graphene two-dimensional nanosheets and the modified matrix material to achieve a high-density nucleobase pair interfacial hydrogen bonds, thereby achieving The parallel arrangement of modified graphene two-dimensional nanosheets forms a bionic anti-naphthalene structure.

Benefits of technology

A self-repair material with excellent mechanical strength, tensibility and rapid self-repair ability under room temperature and low temperature environments is realized. The mechanical tensile strength is 10~50MPa, the elongation of break is 1000~1800%, and cut into two sections. The ultimate tensile strength is restored by 60% to 90%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019837A_ABST
    Figure CN119019837A_ABST
Patent Text Reader

Abstract

The invention provides a self-repairing material based on nucleobase pair assembly as well as a preparation method and application of the self-repairing material. The self-repairing material comprises a modified matrix material and a modified graphene two-dimensional nanosheet embedded in the modified matrix material, the modified graphene two-dimensional nanosheet comprises graphene oxide modified by a modifier containing dynamic hydrogen bonds; the modified matrix material comprises a matrix material modified by a sextuple hydrogen bond-containing monomer and / or a nucleobase chain extender. In the self-repairing material provided by the invention, due to the existence of high-density nucleobase pair hydrogen bonds on an interface between the modified graphene two-dimensional nanosheets and the polyurethane matrix material, the graphene two-dimensional nanosheets are arranged in the polyurethane matrix material in a parallel arrangement manner, and the self-repairing material has a bionic anti-pearl layer structure; therefore, the mechanical strength of the self-repairing material is improved, and the self-repairing material has excellent tensile property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of self-repairing coatings, and in particular to a self-repairing material assembled by nucleobase pairs, and a preparation method and application thereof. Background Art

[0002] Self-healing supramolecular elastomers have attracted considerable attention due to their characteristics of autonomously repairing material damage defects to restore their original functions, being recyclable and reducing environmental burdens. They are widely used in artificial electronic skin, flexible robots, and wearable electronic devices. The polymer damage repair ability of supramolecular polyurethanes is usually achieved through the reversible dynamic bonds of cross-linked molecular chains or the physical structure of the polymer network, including covalent or non-covalent hydrogen bonds, imine bonds, metal-ligand coordination, disulfide and Diels-Alder (DA) reactions. However, most of these self-healing elastomers require specific stimuli such as molecular changes, light changes, or temperature changes to achieve functional repair. The prior art proposes an effective strategy to introduce non-covalent hydrogen bonding interactions into molecular chains as reversible cross-linking bonds and sacrificial bonds to prepare tough and room temperature self-healing materials. However, due to the inherent contradiction between the mechanical strength and self-healing ability of the material caused by weak non-covalent bonds, such materials usually exhibit limited ultimate tensile strength and low elongation. Therefore, how to balance the contradiction between the mechanical strength, tensile properties and rapid room temperature self-healing ability of self-healing materials is a major challenge. This is because the high mechanical properties of the material come from different molecular mechanisms in the molecular rigidity organization, while the self-healing ability depends on the dynamic breakage and reconstruction of molecular chains, so they are usually mutually exclusive.

[0003] In nature, biomacromolecules based on non-covalent self-assembly, such as spider silk and nacre, exhibit an extraordinary combination of contradictory mechanical properties and a certain self-healing ability after damage. The small-sized β-sheet nanocrystals composed of dense hydrogen bond motifs and polypeptide chains in spider silk are uniformly embedded in the amorphous matrix. The dynamic hydrogen bond break-reorganization caused by external forces can dissipate a lot of energy, making it one of the strongest materials found in nature. The special "brick-mud" structure of natural nacre, which has evolved for centuries, consists of 4wt.% biopolymers and about 96wt.% inorganic sheets, showing extremely high strength, toughness and stability. Loading rigid inorganic nanofillers is the main means to improve the mechanical strength of polymers. Although this method can achieve efficient enhancement of the mechanical properties of low-strength polymer materials, the introduction of nanofillers restricts the movement of polymer segments, the self-healing performance is limited, and it is difficult to achieve high tensile properties; that is, the self-healing material system in the prior art cannot simultaneously meet the contradiction between high mechanical properties, tensile properties and rapid self-healing ability. Therefore, it is of great significance to design self-healing coatings that have high mechanical strength, excellent tensile properties and rapid room temperature self-healing ability.

[0004] In view of the problems existing in the above-mentioned prior art, the present invention provides a self-healing material assembled by nucleobase pairs and a preparation method and application thereof. A self-healing coating assembled by nucleobase pairs is prepared by synergistically combining main chain hydrogen bonds, side chain hydrogen bonds and interface hydrogen bonds. The self-healing coating can not only achieve self-repair under room temperature conditions, but also has the ability to self-repair under low temperature and / or water environment. Summary of the invention

[0005] In view of this, the technical problem to be solved by the present invention is to provide a self-healing material assembled by nucleobase pairs and a preparation method and application thereof, which successfully balances the contradictions among high mechanical properties, excellent stretchability and rapid room temperature self-healing ability in the self-healing material system, so that it can be applied to the field of metal corrosion protection or flexible crawling robots.

[0006] In order to achieve the above-mentioned object, the present invention provides a self-healing material based on nucleobase pair assembly, comprising a modified matrix material and a modified graphene two-dimensional nanosheet; wherein the modified graphene two-dimensional nanosheet comprises graphene oxide modified by a modifier containing dynamic hydrogen bonds; the modified matrix material comprises a matrix material modified by a monomer containing a sextuple hydrogen bond and / or a nucleobase chain extender. Moreover, the interface between the modified graphene two-dimensional nanosheet and the modified matrix material forms an interface hydrogen bond of nucleobase pairs, so that the modified graphene two-dimensional nanosheet is arranged in parallel in the modified matrix material, thereby making the self-healing material have a bionic anti-pearl structure.

[0007] Preferably, the modifier containing dynamic hydrogen bonds and the nucleobase extender respectively contain complementary paired bases for forming the nucleobase pair.

[0008] Furthermore, the nucleobase pair includes, but is not limited to, any one of a combination of thymine and adenine (T=A), a combination of cytosine and guanine (C=G), and a combination of uracil and adenine (U=A).

[0009] Preferably, the modifier containing dynamic hydrogen bonds comprises any one of the nucleobases thymine, cytosine, uracil, adenine and guanine.

[0010] Preferably, the nucleobase chain extender is at least selected from monomers containing pyrimidines or monomers containing purines.

[0011] More preferably, the pyrimidine monomer comprises any one of thymine, cytosine and uracil.

[0012] More preferably, the purine monomer includes any one of adenine and guanine.

[0013] Preferably, the monomer containing a sextuple hydrogen bond comprises adipic acid dihydrazide.

[0014] Preferably, the modified matrix material contains multiple types of hydrogen bonds, and the multiple types of hydrogen bonds include a combination of two or three of main chain hydrogen bonds, side chain hydrogen bonds, and interface hydrogen bonds.

[0015] Preferably, the energy diffusion mechanism constructed by the breaking-movement-reconstruction of the multi-type hydrogen bonds enables the room temperature self-healing material to have a self-healing function at room temperature, low temperature or in water environment.

[0016] More preferably, the low temperature is -2°C to 5°C.

[0017] Preferably, the main chain hydrogen bonds are obtained by introducing adipic acid dihydrazide monomer containing a hexaplethic hydrogen bond into the matrix material.

[0018] Preferably, the side chain hydrogen bonds are produced by the nucleobase chain extender in the matrix material.

[0019] Preferably, the interfacial hydrogen bonds are formed by embedding the modified graphene two-dimensional nanosheets in the matrix material to form an interface.

[0020] Preferably, the preparation method of the modified graphene two-dimensional nanosheet comprises: adding the modifier containing dynamic hydrogen bonds to the graphene oxide dispersion activated by N,N′-carbonyldiimidazole (CDI), and stirring at 20 to 80° C. for 4 to 12 hours to obtain the modified graphene two-dimensional nanosheet.

[0021] Preferably, the mass ratio of the modifier containing dynamic hydrogen bonds to graphene oxide is 1:10 to 100:1.

[0022] More preferably, the mass ratio of CDI to graphene oxide in the CDI-activated graphene oxide dispersion is 10:1 to 100:1.

[0023] Preferably, the graphene oxide dispersion is a 0.1-10 mg / mL graphene oxide / water dispersion.

[0024] Preferably, the graphene oxide has a diameter of 0.5 to 15 μm and a thickness of 0.7 to 10 nm.

[0025] Preferably, the repair function of the self-repairing material includes self-repairing of mechanical properties and / or self-repairing of salt water corrosion protection function and / or self-repairing of photothermal response creeping function.

[0026] Preferably, the self-repair of the mechanical property is that the tensile strength of the material is restored by 70% to 90%.

[0027] As another purpose, the present invention also provides a method for preparing the above-mentioned self-healing material based on nucleobase pair assembly. An embodiment of the present invention also provides a method for preparing a room-temperature self-healing coating assembled by nucleobase pairs, which comprises: introducing two or more combinations of the main chain hydrogen bonds, side chain hydrogen bonds, and interface hydrogen bonds into a prepolymer obtained after the reaction of polyol and diisocyanate to obtain a polyurethane material, and then adding modified graphene two-dimensional nanosheets, and due to the presence of high-density interfacial nucleobase pair hydrogen bonds, the modified graphene two-dimensional nanosheets are arranged in the polyurethane in a parallel arrangement to obtain a composite material with a bionic anti-pearl structure.

[0028] Specifically, the steps include:

[0029] S1. Providing a modified matrix material;

[0030] Introducing one or both of main chain hydrogen bonds and side chain hydrogen bonds into the prepolymer of the matrix material to obtain the modified matrix material;

[0031] S2. providing modified graphene two-dimensional nanosheets;

[0032] Adding a modifier containing dynamic hydrogen bonds to the graphene oxide dispersion after CDI activation, stirring and reacting to obtain the modified graphene two-dimensional nanosheet;

[0033] S3. Preparation of self-healing materials;

[0034] The modified graphene two-dimensional nanosheet and the modified matrix material are mixed and stirred for reaction to obtain the self-healing material.

[0035] As a preferred embodiment, in S1, the base material is polyurethane; the preparation method of the modified base material comprises blending a polyol, a diisocyanate and an organic solvent, and stirring at 60 to 100° C. for 2 to 5 hours to obtain a prepolymer; adding one or a combination of adipic acid dihydrazide and a nucleobase chain extender to the prepolymer and stirring at 30 to 70° C. for 2 to 20 hours to obtain a polyurethane material.

[0036] Preferably, the diisocyanate comprises one of dicyclohexylmethane diisocyanate (HMDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), and hexamethylene diisocyanate (HDI).

[0037] Preferably, the polyol comprises at least one of polytetramethylene glycol (PTMEG), 1,4-butanediol (BDO), and polypropylene glycol (PPG).

[0038] Preferably, the organic solvent comprises at least one of N,N-dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), and N,N-dimethylformamide (DMF).

[0039] Preferably, the mass ratio of the polyol to the organic solvent is 2:1 to 1:5.

[0040] Preferably, the molar ratio of the polyol to the diisocyanate is 1:1 to 1:2.

[0041] Preferably, the molar ratio of the polyol to one or a combination of adipic acid dihydrazide and a nucleobase chain extender is 1:1.

[0042] In S2, the mass ratio of the modifier containing dynamic hydrogen bonds to the graphene oxide is 1:10 to 100:1.

[0043] Preferably, in the graphene oxide dispersion after CDI activation, the mass ratio of CDI to graphene oxide is 10:1 to 100:1.

[0044] Preferably, the graphene oxide dispersion after CDI activation is a 0.1-10 mg / mL graphene oxide / water dispersion; wherein the graphene oxide has a diameter of 0.5-15 μm and a thickness of 0.7-10 nm.

[0045] Preferably, in S3, the mass ratio of the modified matrix material to the modified graphene two-dimensional nanosheets is 2000:1 to 20:1.

[0046] Preferably, the mixing temperature is 25-50° C., and the stirring reaction time is 0.5-5 h.

[0047] As one of the objects of the invention, the present invention also provides a self-healing coating obtained by curing the above-mentioned self-healing material based on nucleobase pair assembly; preferably, the curing temperature is 40-100°C and the time is 10-60h.

[0048] Based on the above technical scheme, the self-healing material assembled by the nucleobase pairs disclosed in the present invention is formed by connecting multiple types of hydrogen bonds, wherein the multiple types of hydrogen bonds are a combination of main chain hydrogen bonds, side chain hydrogen bonds, and interface hydrogen bonds, and the nucleobase pairs are one of thymine and adenine (T=A), cytosine and guanine (C=G), and uracil and adenine (U=A). The preparation method comprises: introducing the side chain containing the above-mentioned pyrimidine or purine monomer into the main chain containing adipic acid dihydrazide monomer, and finally introducing the graphene two-dimensional nanosheet modified by the monomer corresponding to the above-mentioned nucleobase pair. Due to the presence of interfacial nucleobase pair hydrogen bonds, the modified graphene two-dimensional nanosheet of the present invention can be arranged in parallel in polyurethane. The prepared room temperature self-healing coating assembled by the nucleobase pairs exhibits excellent mechanical strength, stretchability, and rapid room temperature, low temperature, and water environment self-healing ability due to the synergistic effect of side chain hydrogen bonds, multiple dynamic hydrogen bonds, and interfacial base pair hydrogen bonds.

[0049] Beneficial technical effects obtained by the present invention:

[0050] (1) In the self-healing material provided by the technical solution of the present invention, due to the presence of high-density nucleobase hydrogen bonds at the interface between the modified graphene two-dimensional nanosheets and the polyurethane matrix material, the graphene two-dimensional nanosheets are arranged in a parallel arrangement in the polyurethane matrix, thereby improving the mechanical strength of the material and having excellent stretchability; its mechanical tensile strength is 10 to 50 MPa, and the elongation at break is 1000 to 1800%.

[0051] (2) The self-healing material assembled by nucleobase pairs provided by the present invention has a rapid self-healing ability at room temperature, low temperature (~2°C) and water environment due to the energy diffusion mechanism constructed by the breaking-movement-reconstruction of multiple types of hydrogen bonds in the matrix material.

[0052] (3) The room temperature self-healing material assembled by the nucleobase pairs provided by the present invention can recover 60% to 90% of its ultimate tensile strength after being cut into two sections and kept in contact at room temperature for 0.5 to 12 hours. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 is a schematic diagram of the synthesis process of the polyurethane material obtained in Example 1 of the present invention;

[0054] Figure 2 is a scanning electron microscope image of the room temperature self-healing coating assembled by nucleobase pairs described in Example 1 of the present invention comprising parallel arranged two-dimensional nanosheets;

[0055] Figure 3 is a tensile test stress-strain curve of the room temperature self-healing coating assembled by nucleobase pairs prepared in Example 1 of the present invention;

[0056] Figure 4This is a scanning electron microscope image of the room temperature self-healing coating assembled by the nucleobase pairs prepared in Example 1 of the present invention after being cut into two sections and contacted at room temperature for 2 hours;

[0057] Figure 5 is a tensile test stress-strain curve of the room temperature self-healing coating assembled by the nucleobase pairs prepared in Example 1 of the present invention after being sheared into two sections and contacted at room temperature for 2 hours;

[0058] Figure 6 It is a local electrochemical impedance diagram of the self-repairing behavior of the room temperature self-repairing coating assembled by the nucleobase pairs prepared in Example 1 of the present invention in 3.5wt.% sodium chloride ice brine (~2°C);

[0059] Figure 7 This is an optical photograph of the crawling process of a crawling robot under infrared light after being repaired at room temperature for 2 hours by the room temperature self-healing coating assembled by the nucleobase pairs prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0060] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application will be clearly and completely described below in combination with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments.

[0061] One aspect of the present invention provides a room temperature self-healing coating that imitates natural spider silk and pearl layer structure based on nucleobase pair driven assembly, which is formed by a combination of main chain hydrogen bonds, side chain hydrogen bonds, and interface hydrogen bonds, wherein the interface between modified graphene two-dimensional nanosheets and polyurethane is arranged in parallel in the polyurethane due to the presence of high-density nucleobase pair hydrogen bonds.

[0062] In some preferred embodiments, the modified graphene two-dimensional nanosheet is made of graphene oxide modified by one of the nucleobases thymine, cytosine, uracil, adenine and guanine.

[0063] In some preferred embodiments, the method for preparing the modified graphene two-dimensional nanosheets includes: adding a modifier containing dynamic hydrogen bonds to a graphene oxide dispersion activated by N,N′-carbonyldiimidazole (CDI), and stirring at 20 to 80° C. for 4 to 12 hours to obtain modified graphene two-dimensional nanosheets.

[0064] Furthermore, the modifier containing dynamic hydrogen bonds is one of the above-mentioned nucleobases thymine, cytosine, uracil, adenine, and guanine.

[0065] Furthermore, the mass ratio of the modifier to graphene oxide is 1:10 to 100:1.

[0066] Furthermore, the mass ratio of CDI to graphene oxide in the graphene oxide dispersion after CDI activation is 10:1 to 100:1.

[0067] Furthermore, the graphene oxide dispersion is a 0.1-10 mg / mL graphene oxide / water dispersion.

[0068] Furthermore, the graphene oxide has a diameter of 0.5 to 15 μm and a thickness of 0.7 to 10 nm.

[0069] Another aspect of an embodiment of the present invention provides a method for preparing a self-healing material, comprising: introducing two or more combinations of the main chain hydrogen bonds, side chain hydrogen bonds, and interface hydrogen bonds into a prepolymer obtained after the reaction of a polyol and a diisocyanate to obtain a polyurethane material.

[0070] In some preferred embodiments, the reaction conditions of the preparation method include: mixing a polyol, a diisocyanate and an organic solvent, and stirring at 60-100° C. for 2-5 hours to obtain a prepolymer; adding one or a combination of adipic acid dihydrazide and a nucleobase chain extender to the prepolymer and stirring at 30-70° C. for 2-20 hours to obtain a polyurethane material.

[0071] Furthermore, the diisocyanate comprises one of dicyclohexylmethane diisocyanate (HMDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), and hexamethylene diisocyanate (HDI).

[0072] Furthermore, the polyol comprises at least one of polytetramethylene glycol (PTMEG), 1,4-butanediol (BDO), and polypropylene glycol (PPG).

[0073] In some preferred embodiments, the organic solvent includes at least one of N,N-dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), and N,N-dimethylformamide (DMF).

[0074] Furthermore, the mass ratio of the polyol to the organic solvent is 2:1 to 1:5.

[0075] Furthermore, the molar ratio of the polyol to the diisocyanate is 1:1 to 1:2.

[0076] Furthermore, the molar ratio of the polyol to one or a combination of adipic acid dihydrazide and a nucleobase chain extender is 1:1.

[0077] Another aspect of an embodiment of the present invention provides a method for preparing a room temperature self-healing coating assembled by nucleobase pairs, comprising: adding modified graphene two-dimensional nanosheets to the above polyurethane solution, and arranging the modified graphene two-dimensional nanosheets in the polyurethane in a parallel arrangement due to the presence of high-density nucleobase pair hydrogen bonds at the interface, thereby obtaining a composite material having a bionic anti-pearl structure;

[0078] The composite coating is cured to obtain the room temperature self-healing coating assembled by the nucleobase pairs.

[0079] Furthermore, the mass ratio of the polyurethane material to the modified graphene two-dimensional nanosheets is 2000:1 to 20:1.

[0080] Furthermore, the mixing temperature is 25-50° C., and the stirring time is 0.5-5 h.

[0081] In some preferred embodiments, the curing temperature is 40-100° C. and the curing time is 10-60 hours.

[0082] In some preferred embodiments, the room temperature self-healing coating assembled by nucleobase pairs has rapid room temperature functional self-healing ability due to the energy diffusion mechanism constructed by the breakage-movement-reconstruction of multiple types of hydrogen bonds in polyurethane.

[0083] In some more typical specific implementation cases, a method for preparing a room temperature self-healing coating assembled by nucleobase pairs of the present invention comprises the following steps:

[0084] 1) Modification of graphene two-dimensional nanosheets: Add a modifier containing dynamic hydrogen bonds in a mass ratio of 1:10 to 100:1 to a CDI-activated graphene oxide dispersion and stir at 20 to 80° C. for 4 to 12 hours.

[0085] 2) Preparation of self-healing polyurethane material: polyol, diisocyanate and organic solvent are mixed and stirred at 60-100° C. for 2-5 hours to obtain a prepolymer; adipic acid dihydrazide and a nucleobase chain extender or a combination thereof are added to the prepolymer and stirred at 30-70° C. for 2-20 hours to obtain a polyurethane material.

[0086] 3) Preparation of room temperature self-healing coating assembled by nucleobase pairs: Mix a polyurethane solution and modified graphene two-dimensional nanosheets in a mass ratio of 2000:1 to 20:1, stir at 25 to 50°C for 0.5 to 5h to obtain a nacreous layer structure self-healing material, and finally cure the composite material to obtain a room temperature self-healing coating assembled by nucleobase pairs; wherein the curing temperature is 40 to 100°C and the time is 10 to 60h.

[0087] The embodiment of the present invention also provides a room temperature self-healing coating assembled by nucleobase pairs prepared by the aforementioned method.

[0088] The embodiments of the present invention also provide the use of the room temperature self-repairing coating assembled by the aforementioned nucleobase pairs in the preparation of a metal corrosion protection structure or a flexible crawling robot.

[0089] In summary, the present invention prepares a room temperature self-healing coating assembled by nucleobase pairs by synergistically combining a combination of main chain hydrogen bonds, side chain hydrogen bonds, and interface hydrogen bonds. Among them, the modified graphene two-dimensional nanosheets can be arranged in a parallel arrangement in polyurethane due to the presence of high-density nucleobase pair hydrogen bonds at the interface. The room temperature self-healing coating assembled by nucleobase pairs has high mechanical strength due to the presence of parallel arranged nanosheets, and at the same time, it has excellent stretchability due to the presence of multiple types of hydrogen bonds. With the help of the energy diffusion mechanism of the break-move-reconstruction of multiple types of hydrogen bonds in polyurethane, it has a rapid room temperature functional self-healing ability; specifically, the mechanical tensile strength of the room temperature self-healing coating assembled by nucleobase pairs is 10-50MPa, and the elongation at break is 1000-1800%; and the ultimate tensile strength of the polyurethane coating cut into two sections can be restored by 60%-90% after contact at room temperature for 0.5-12h. The contradiction between high mechanical properties, excellent stretchability and rapid room temperature self-healing ability in the self-healing material system is successfully balanced.

[0090] It should be noted that, unless otherwise specified, the raw materials and chemical reagents used in the present invention are all commercially available.

[0091] The technical solutions in the embodiments of the present invention are clearly and completely described below through specific embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0092] Example 1

[0093] This embodiment provides a method for preparing a room temperature self-healing coating assembled by nucleobase pairs, which is described below using polyurethane as an example of a base material.

[0094] See also Figure 1 , which is a schematic diagram of the preparation process of the self-healing material. As shown in the figure, PTMEG (polytetramethylene glycol, molecular weight 2000g / mol), HMDI (dicyclohexylmethane diisocyanate) and are stirred at 80°C for 3h under nitrogen protection to obtain a prepolymer; adipic acid dihydrazide and a thymine-containing nucleobase chain extender are added to the prepolymer to react to obtain a modified polyurethane material; the modified polyurethane material is mixed with modified graphene to obtain a self-healing material with nucleobase pair assembly.

[0095] Specifically, the preparation method comprises the following steps:

[0096] 1. Modification of graphene two-dimensional nanosheets: A 1.2:1 mass ratio of adenine modifier containing dynamic hydrogen bonds was added to a 2 mg / mL CDI (N, N′-carbonyldiimidazole) activated graphene oxide dispersion and stirred at 60°C for 8 h, wherein the CDI:graphene oxide mass ratio was 27:1;

[0097] The preparation method of CDI activated graphene oxide includes: taking 1.6g of graphene nanosheets (GO nanosheets) and dispersing them in 800ml DMF, and ultrasonically dispersing them in a water bath for 20 minutes. Then adding 43.24g of N, N′-carbonyldiimidazole (CDI), and stirring at 60°C for 12h. The obtained suspension is centrifuged at 10000rpm for 10 minutes, and washed with ethanol, deionized water and DMF for 3 times respectively to obtain CDI activated graphene oxide; the surface of the obtained CDI activated graphene oxide contains a large number of oxygen-containing functional groups (such as carboxyl -COOH), so as to complete the grafting of adenine modifiers containing dynamic hydrogen bonds in the subsequent step.

[0098] 2. Preparation of self-healing polyurethane material: 80g PTMEG (polytetramethylene glycol, molecular weight 2000g / mol, 40mmol), 21g HMDI (dicyclohexylmethane diisocyanate, 80mmol) and 200mL DMAc (N,N-dimethylacetamide) were blended and stirred at 80°C for 3h to obtain a prepolymer; 3.484g adipic acid dihydrazide (20mmol) and a thymine-containing nucleobase extender (20mmol, thymine-1-acetic acid, CAS: 20924-05-4, Aladdin, catalog number: T130008) were added to the prepolymer and stirred at 80°C for 3h to obtain a polyurethane material.

[0099] 3. Preparation of room temperature self-healing material assembled by nucleobase pairs: Modified graphene two-dimensional nanosheets were mixed in a polyurethane solution with a mass ratio of 200:1 and stirred at 40°C for 3 h to obtain a self-healing material with a nacre-like structure.

[0100] 4. Preparation of self-healing coating: The self-healing material prepared in the above steps was cured at 80°C for 36 hours to obtain a room temperature self-healing coating assembled by nucleobase pairs.

[0101] like Figure 2 The figure shows a scanning electron microscope image of the self-healing material assembled by the nucleobase pairs provided in this embodiment, in which the polyurethane contains parallel-arranged two-dimensional nanosheets. Obviously, the modified graphene two-dimensional nanosheets are arranged in parallel in the polyurethane, which is conducive to improving the mechanical strength of the self-healing material. At the same time, due to the presence of high-density nucleobase pair hydrogen bonds at the polyurethane / graphene interface, it has excellent stretchability.

[0102] See also Figure 3 , is the tensile test stress-strain curve of the self-healing material in this embodiment. It can be seen from the figure that its mechanical tensile strength and elongation at break are 46.6MPa and 1736.9% respectively, showing excellent mechanical properties.

[0103] Furthermore, after the self-healing material was cut into two pieces and kept in contact at room temperature for 2 hours, its tensile strength could recover by 85.6%, indicating that the energy diffusion mechanism of the break-move-reconstruction of the main chain hydrogen bonds, side chain hydrogen bonds, and interface hydrogen bonds in the polyurethane material of this embodiment has the rapid room temperature functional self-healing ability.

[0104] See also Figure 4 and Figure 5 , respectively, are the scanning electron microscope image of the self-healing material after shearing for 2 hours and the stress-strain curve of the tensile test.

[0105] Furthermore, this example also examines the self-healing ability of the self-healing coating after 2 h in low temperature (~2°C) and 3.5wt.% salt water. Figure 6 As shown, autonomous healing can be achieved even at low temperature and 3.5wt.% salt water, demonstrating outstanding self-healing capabilities in water environment and at low temperature.

[0106] By taking advantage of the difference in thermal expansion coefficients between the self-healing coating and the modified graphene two-dimensional nanosheets described in this embodiment, a crawling robot was assembled, which can exhibit crawling behavior under the drive of near-infrared light. The optical process is as follows: Figure 7 shown.

[0107] In summary, the room temperature self-healing coating assembled by nucleobase pairs prepared in this embodiment has broad application prospects in the fields of metal corrosion protection, flexible crawling robots and the like.

[0108] Example 2

[0109] This embodiment provides a method for preparing a room temperature self-healing coating assembled by nucleobase pairs, comprising the following steps:

[0110] 1. Modification of graphene two-dimensional nanosheets: Add a cytosine modifier containing dynamic hydrogen bonds at a mass ratio of 1:10 to a 0.1 mg / mL CDI-activated graphene oxide dispersion and stir at 20°C for 12 h, wherein the mass ratio of CDI to graphene oxide is 10:1;

[0111] 2. Preparation of self-healing polyurethane material: BDO (1,4-butanediol, 40 mmol), TDI (toluene diisocyanate, 80 mmol) and 100 mL DMSO (dimethyl sulfoxide) were mixed and stirred at 60°C for 5 h to obtain a prepolymer; 1.742 g of adipic acid dihydrazide (10 mmol) and a guanine-containing nucleobase chain extender (30 mmol, guanine nucleoside, CAS No.: 118-00-3, Aladdin, Catalog No.: G103965) were added to the prepolymer and stirred at 30°C for 20 h to obtain a polyurethane material.

[0112] 3. Preparation of room-temperature self-healing coating assembled by nucleobase pairs: Mix modified graphene two-dimensional nanosheets in a polyurethane solution with a mass ratio of 2000:1, stir at 25°C for 5 hours to obtain a nacre-like structure self-healing material, and finally cure the composite material at 40°C for 60 hours to obtain a room-temperature self-healing coating assembled by nucleobase pairs.

[0113] The self-repairing performance of the self-repairing polyurethane material prepared in this embodiment is similar to that in embodiment 1.

[0114] Example 3

[0115] This embodiment provides a method for preparing a room temperature self-healing coating assembled by nucleobase pairs, comprising the following steps:

[0116] 1. Modification of graphene two-dimensional nanosheets: A guanine modifier containing dynamic hydrogen bonds at a mass ratio of 100:1 was added to a 10 mg / mL CDI-activated graphene oxide dispersion and stirred at 80°C for 4 h, wherein the mass ratio of CDI:graphene oxide was 100:1.

[0117] 2. Preparation of self-healing polyurethane material: PPG (polypropylene glycol, molecular weight 2000 g / mol, 40 mmol), IPDI (isophorone diisocyanate, 80 mmol) and 250 mL DMF (N, N-dimethylformamide) were blended and stirred at 100 °C for 2 h to obtain a prepolymer; 5.226 g of adipic acid dihydrazide (30 mmol) and a cytosine-containing nucleobase extender (10 mmol, N4-acetylcytosine, CAS No.: 14631-20-0, Aladdin, Product No.: N103229) were added to the prepolymer and stirred at 70 °C for 2 h to obtain a polyurethane material.

[0118] 3. Preparation of room-temperature self-healing coating assembled by nucleobase pairs: Mix modified graphene two-dimensional nanosheets in a polyurethane solution with a mass ratio of 20:1, stir at 50°C for 0.5h to obtain a nacreous layer structure self-healing material, and finally cure the self-healing material at 100°C for 10h to obtain a self-healing coating assembled by nucleobase pairs.

[0119] Example 4

[0120] This embodiment provides a method for preparing a room temperature self-healing coating assembled by nucleobase pairs, comprising the following steps:

[0121] 1. Modification of graphene two-dimensional nanosheets: A 50:1 mass ratio of uracil modifier containing dynamic hydrogen bonds was added to a 5 mg / mL CDI-activated graphene oxide dispersion and stirred at 40°C for 6 h, wherein the CDI:graphene oxide mass ratio was 50:1.

[0122] 2. Preparation of self-healing polyurethane material: PTMEG (molecular weight 1000 g / mol, 40 mmol), MDI (4,4'-diphenylmethane diisocyanate, 80 mmol) and 150 mL DMF+DMAc were blended and stirred at 70 °C for 4 h to obtain a prepolymer; 2.613 g of adipic acid dihydrazide (15 mmol) and an adenine-containing nucleobase extender (25 mmol, adenine nucleoside, CAS No.: 58-61-7, Aladdin, Product No.: A108806) were added to the prepolymer and stirred at 50 °C for 10 h to obtain a polyurethane material.

[0123] 3. Preparation of room-temperature self-healing coating assembled by nucleobase pairs: Mix modified graphene two-dimensional nanosheets in a polyurethane solution with a mass ratio of 1000:1, stir at 30°C for 4 hours to obtain a nacre-like structure self-healing material, and finally cure the composite material at 70°C for 40 hours to obtain a room-temperature self-healing coating assembled by nucleobase pairs.

[0124] Example 5

[0125] This embodiment provides a method for preparing a room temperature self-healing coating assembled by nucleobase pairs, comprising the following steps:

[0126] 1. Modification of graphene two-dimensional nanosheets: A thymine modifier containing dynamic hydrogen bonds at a mass ratio of 20:1 was added to a 1 mg / mL CDI-activated graphene oxide dispersion and stirred at 50°C for 10 h, wherein the mass ratio of CDI:graphene oxide was 20:1.

[0127] 2. Preparation of self-healing polyurethane material: PPG (molecular weight 1000 g / mol, 40 mmol), HDI (80 mmol) and 200 mL DMSO+DMAc were blended and stirred at 90°C for 2.5 h to obtain a prepolymer; 4.355 g adipic acid dihydrazide (25 mmol) and an adenine-containing nucleobase extender (15 mmol, adenine nucleoside, CAS No.: 58-61-7, Aladdin, Catalog No.: A108806) were added to the prepolymer and stirred at 40°C for 12 h to obtain a polyurethane material.

[0128] 3. Preparation of room-temperature self-healing coating assembled by nucleobase pairs: Mix modified graphene two-dimensional nanosheets in a polyurethane solution with a mass ratio of 500:1, stir at 45°C for 2 hours to obtain a nacre-like structure self-healing material, and finally cure the composite material at 60°C for 50 hours to obtain a room-temperature self-healing coating assembled by nucleobase pairs.

[0129] The mechanical properties of Examples 2 to 5 were tested respectively. Similar to Example 1, the mechanical tensile strength was 10 to 50 MPa, and the elongation at break was 1000 to 1800%. The polyurethane coating cut into two sections could recover 60% to 90% of its ultimate tensile strength after contact at room temperature for 0.5 to 12 hours, and could also achieve self-healing at low temperature and 3.5wt.% saline. Therefore, the technical scheme of Examples 2 to 5 can also achieve the same technical effect as Example 1.

[0130] Comparative Example 1

[0131] This comparative example provides a method for preparing a room temperature self-healing polyurethane material, comprising the following steps:

[0132] 80 g of PTMEG (molecular weight 2000 g / mol, 40 mmol), 21 g of HMDI (80 mmol) and 200 mL of DMAc were blended and stirred at 80° C. for 3 h to obtain a prepolymer; 3.484 g of adipic acid dihydrazide (20 mmol) and a thymine-containing nucleobase chain extender (20 mmol) were added to the prepolymer and stirred at 40° C. for 12 h to obtain a polyurethane material.

[0133] The ultimate tensile strength and elongation of the prepared polyurethane material were 59.6MPa and 1112.4% respectively, but it could not self-repair at room temperature. At 80°C, the mechanical strength of the material broken into two pieces could be restored to 53.8MPa after 2h of contact, and the mechanical strength repair efficiency was 90.3%.

[0134] Comparative Example 2

[0135] This comparative example provides a method for preparing a room temperature self-healing polyurethane material, comprising the following steps:

[0136] BDO (40 mmol), TDI (80 mmol) and 100 mL DMSO were mixed and stirred at 60° C. for 5 h to obtain a prepolymer; 1.742 g adipic acid dihydrazide (10 mmol) and a guanine-containing nucleobase chain extender (30 mmol) were added to the prepolymer and stirred at 30° C. for 20 h to obtain a polyurethane material.

[0137] The results of this comparative example are similar to those of comparative example 1, and this comparative example also does not have the self-repairing function at room temperature.

[0138] Comparative Example 3

[0139] This comparative example provides a method for preparing a room temperature self-healing polyurethane material, comprising the following steps:

[0140] PPG (molecular weight 2000 g / mol, 40 mmol), IPDI (80 mmol) and 250 mL DMF were blended and stirred at 100° C. for 2 h to obtain a prepolymer; 5.226 g of adipic acid dihydrazide (30 mmol) and a cytosine-containing nucleobase extender (10 mmol) were added to the prepolymer and stirred at 70° C. for 2 h to obtain a polyurethane material.

[0141] The results of this comparative example are similar to those of comparative example 1, and this comparative example also does not have the self-repairing function at room temperature.

[0142] In summary, the present invention prepares a room temperature self-healing coating assembled by nucleobase pairs by synergistically combining a combination of main chain hydrogen bonds, side chain hydrogen bonds, and interface hydrogen bonds. Among them, the modified graphene two-dimensional nanosheets can be arranged in a parallel arrangement in polyurethane due to the presence of high-density nucleobase pair hydrogen bonds at the interface. The room temperature self-healing coating assembled by nucleobase pairs has high mechanical strength due to the presence of parallel arranged nanosheets, and at the same time, it has excellent stretchability due to the presence of multiple types of hydrogen bonds. With the help of the energy diffusion mechanism of the break-move-reconstruction construction of multiple types of hydrogen bonds in polyurethane, it has a rapid room temperature functional self-healing ability; specifically, the mechanical tensile strength of the room temperature self-healing coating assembled by nucleobase pairs is 10-50MPa, and the elongation at break is 1000-1800%; and the ultimate tensile strength of the polyurethane coating cut into two sections can be restored by 60%-90% after contact at room temperature for 0.5-12h. The self-healing material obtained by the technical solution of the present invention successfully balances the contradictions between high mechanical properties, excellent stretchability and rapid room temperature self-healing ability in the self-healing material system.

[0143] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.

[0144] The use of headings and description contents in the present invention is not meant to limit the invention; each section can be applied to any aspect, embodiment or feature of the invention.

[0145] Throughout the present disclosure, where a composition is described as having, comprising, or including particular components, or where a process is described as having, comprising, or including particular process steps, it is contemplated that the compositions taught by the present invention also consist essentially of, or consist of, the recited components, and that the processes taught by the present invention also consist essentially of, or consist of, the recited process steps.

[0146] Unless specifically stated otherwise, use of the terms "include," "includes," "including," "have," "has," or "having" should generally be construed as open ended and non-limiting.

[0147] It should be understood that the order of the various steps or the order in which a particular action is performed is not very important, as long as the teachings of the present invention remain operable. In addition, two or more steps or actions may be performed simultaneously.

[0148] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0149] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made without departing from the spirit and scope of the present invention and that the elements of the embodiments may be replaced by substantial equivalents. In addition, many modifications may be made without departing from the scope of the present invention to adapt specific circumstances or materials to the teachings of the present invention. Therefore, it is not intended herein to limit the present invention to the disclosed specific embodiments for performing the present invention, but it is intended that the present invention will include all embodiments within the scope of the appended claims. In addition, unless specifically stated, any use of the terms first, second, etc. does not indicate any order or importance, but rather uses the terms first, second, etc. to distinguish one element from another.

Claims

1. A self-healing material based on nucleobase pair assembly, characterized in that: It includes a modified matrix material and a modified graphene two-dimensional nanosheet; wherein the modified graphene two-dimensional nanosheet includes graphene oxide modified by a modifier containing dynamic hydrogen bonds; the modified matrix material includes a matrix material modified by a monomer containing a sextuple hydrogen bond and / or a nucleobase chain extender; and an interface between the modified graphene two-dimensional nanosheet and the modified matrix material forms an interface hydrogen bond of nucleobase pairs, so that the modified graphene two-dimensional nanosheet is arranged in parallel in the modified matrix material.

2. The self-healing material based on nucleobase pair assembly according to claim 1, characterized in that: The modifier containing dynamic hydrogen bonds and the nucleobase extender respectively contain complementary paired bases for forming the nucleobase pair; preferably, the nucleobase pair includes any one of a combination of thymine and adenine, a combination of cytosine and guanine, and a combination of uracil and adenine; Preferably, the modifier containing dynamic hydrogen bonds comprises any one of the nucleobases thymine, cytosine, uracil, adenine, and guanine; Preferably, the nucleobase chain extender comprises a pyrimidine-containing monomer or a purine-containing monomer; More preferably, the pyrimidine monomer includes any one of thymine, cytosine, and uracil; More preferably, the purine monomer includes any one of adenine and guanine; Preferably, the monomer containing a sextuple hydrogen bond comprises adipic acid dihydrazide monomer.

3. The self-healing material based on nucleobase pair assembly according to claim 1, characterized in that: The modified matrix material contains multiple types of hydrogen bonds, which include a combination of two or three of main chain hydrogen bonds, side chain hydrogen bonds, and interface hydrogen bonds; The energy diffusion mechanism constructed by the breaking-movement-reconstruction of the multi-type hydrogen bonds enables the self-healing material to have self-healing function at room temperature, low temperature or in water environment; preferably, the low temperature condition is -2°C to 5°C; the water environment is 0 to 5wt.% salt water.

4. The self-healing material based on nucleobase pair assembly according to claim 3, characterized in that: The main chain hydrogen bonds are formed by introducing monomers containing sextuple hydrogen bonds into the matrix material; and / or, the side chain hydrogen bonds are formed by introducing the nucleobase chain extender into the matrix material; And / or, the interfacial hydrogen bonds are formed at the interface between the modified matrix material and the modified graphene two-dimensional nanosheets by embedding the modified graphene two-dimensional nanosheets in the modified matrix material.

5. The self-healing material based on nucleobase pair assembly according to claim 1, characterized in that: The preparation method of the modified graphene two-dimensional nanosheet comprises: adding the modifier containing dynamic hydrogen bonds to the graphene oxide dispersion activated by N,N'-carbonyldiimidazole, and reacting at 20-80° C. for 4-12 hours to obtain the modified graphene two-dimensional nanosheet; Preferably, the mass ratio of the modifier containing dynamic hydrogen bonds to the graphene oxide is 1:10 to 100:1; preferably, in the graphene oxide dispersion, the mass ratio of N,N'-carbonyldiimidazole to graphene oxide is 10:1 to 100:1; preferably, the graphene oxide dispersion contains 0.1 to 10 mg / mL graphene oxide; Preferably, the graphene oxide has a diameter of 0.5 to 15 μm and a thickness of 0.7 to 10 nm.

6. The self-healing coating based on nucleobase pair assembly according to claim 1, characterized in that: The repair function of the self-repairing material includes self-repair of mechanical properties and / or self-repair of salt water corrosion protection function and / or self-repair of photothermal response creeping function; Preferably, the self-repair of the mechanical property is that the tensile strength of the material is restored by 70% to 90%.

7. The method for preparing a self-healing material based on nucleobase pair assembly according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. introducing one or both of the main chain hydrogen bonds and the side chain hydrogen bonds into the prepolymer of the matrix material to obtain a modified matrix material; S2. adding a modifier containing dynamic hydrogen bonds to a dispersion of N,N'-carbonyldiimidazole-activated graphene oxide to react and obtain a modified graphene two-dimensional nanosheet; S3. Mixing and reacting the modified graphene two-dimensional nanosheets and the modified matrix material to obtain the self-healing material.

8. The method for preparing the self-repairing material according to claim 7, characterized in that: In S1, the base material includes polyurethane; preferably, the preparation method of the modified base material includes mixing polyol, diisocyanate and organic solvent, and reacting at 60-100° C. for 2-5 hours to obtain a prepolymer; adding one or a combination of adipic acid dihydrazide and a nucleobase chain extender to the prepolymer and reacting at 30-70° C. for 2-20 hours to obtain a polyurethane material; Preferably, the diisocyanate comprises one of dicyclohexylmethane diisocyanate (HMDI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), and hexamethylene diisocyanate (HDI); Preferably, the polyol comprises at least one of polytetramethylene glycol (PTMEG), 1,4-butanediol (BDO), and polypropylene glycol (PPG); Preferably, the organic solvent comprises at least one of N,N-dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), and N,N-dimethylformamide (DMF); Preferably, the mass ratio of the polyol to the organic solvent is 2:1 to 1:5; Preferably, the molar ratio of the polyol to the diisocyanate is 1:1 to 1:2; Preferably, the molar ratio of the polyol to one or a combination of adipic acid dihydrazide and a nucleobase chain extender is 1:1; In S2, the mass ratio of the modifier containing dynamic hydrogen bonds to the graphene oxide is 1:10 to 100:1; Preferably, in the N,N′-carbonyldiimidazole activated graphene oxide dispersion, the mass ratio of N,N′-carbonyldiimidazole to graphene oxide is 10:1 to 100:1; Preferably, the N,N'-carbonyldiimidazole activated graphene oxide dispersion contains 0.1-10 mg / mL graphene oxide; wherein the graphene oxide has a diameter of 0.5-15 μm and a thickness of 0.7-10 nm. In S3, the mass ratio of the modified matrix material to the modified graphene two-dimensional nanosheet is 2000:1 to 20:1; The mixing temperature is 25-50° C., and the reaction time is 0.5-5 h.

9. A self-repairing coating, characterized in that: The coating is obtained by curing the room temperature self-healing material based on nucleobase pair assembly as described in any one of claims 1 to 6; preferably, the curing temperature is 40 to 100° C. and the curing time is 10 to 60 hours.

10. Use of the self-repairing material based on nucleobase pair assembly according to any one of claims 1 to 6 in the preparation of a metal corrosion protection structure or a flexible crawling robot.

Citation Information

Patent Citations

  • Self-repaired graphene oxide / polyurethane composite material and preparation method thereof

    CN106674996A

  • Bionic environment adaptability self-repairing coating as well as preparation method and application thereof

    CN115216219A

  • Self-healing laminate composition, related articles and related methods

    US20220040730A1

  • Self-healing, self-cleaning omniphobic composition, related articles and related methods

    US20220041787A1