Foam material based on corn straw as well as preparation method and application of foam material

Through specific chemical and physical processes, the porous foam material is prepared using raw materials such as corn stalks, which solves the problem that corn stalks cannot be converted into lightweight, high-strength and good thermal insulation properties in the prior art, and realizes the problem of corn stalks not being converted into foam materials with lightweight, high-strength and good thermal insulation properties. Efficient utilization of agricultural waste and the provision of environmentally friendly materials.

CN119019860AActive Publication Date: 2024-11-26QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411286429.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-26
Estimated Expiration
2044-09-13

AI Technical Summary

Technical Problem

The prior art has not yet been widely reported to convert corn stalks into foam materials with lightweight, high-strength and good thermal insulation properties that meet the needs of industrial applications, resulting in insufficient agricultural waste treatment and resource utilization.

Method used

Through specific chemical and physical processes, the porous foam material is prepared by using raw materials such as corn stalks, foam stabilizers, foaming agents and flocculants, including soaking, slurrying, stirring and drying steps to ensure the light quality of the material. , high porosity and thermal insulation performance.

Benefits of technology

It has achieved the effective conversion of corn stalks into foam materials with lightweight, high strength and good thermal insulation performance. It is suitable for the fields of heat insulation, insulation, packaging and filling materials, reduces environmental pollution, and provides new environmentally friendly materials for the industrial field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005043228810000101
    Figure BDA0005043228810000101
  • Figure BDA0005043228810000111
    Figure BDA0005043228810000111
  • Figure HDA0005043228820000011
    Figure HDA0005043228820000011
Patent Text Reader

Abstract

The invention provides a foam material based on corn straw as well as a preparation method and application of the foam material. The foam material is prepared from the following raw materials in parts by mass: 2-30 parts of corn straws, 0.5-5 parts of a foam stabilizer, 0.01-2 parts of a foaming agent, 0.1-2 parts of a flocculating agent and 50-150 parts of deionized water. Through specific chemical and physical process treatment, the corn straw can be converted into a foam material with a porous structure. The foam material is light in weight, high in strength and good in heat insulation performance, and can be applied to the fields of heat insulation, heat preservation, packaging, filling materials and the like; according to the invention, wastes in agricultural production can be effectively utilized, environmental pollution is reduced, and a novel environment-friendly material is provided for the industrial field; the materials not only improve the additional value of agricultural by-products, but also widen the application range of the materials in the fields of building, packaging, filling materials and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a foam material based on corn stalks and a preparation method and application thereof, belonging to the technical field of environmentally friendly materials. Background Art

[0002] Foam material is a lightweight, highly porous material that can achieve certain specific performance indicators. It has the characteristics of light weight, permeability, high porosity and high contact area, and has gradually become a hot spot in new material research.

[0003] Corn stalks are a byproduct of agricultural production. Large amounts of waste not only cause a waste of resources, but may also cause environmental problems. Traditional treatment methods such as incineration or stacking cause varying degrees of pollution to the environment. The use of corn stalks to prepare foam materials can not only effectively utilize agricultural waste, but also reduce the impact on the environment. Therefore, it is of great significance in resource recycling and environmental protection. The prior art has not widely reported methods for converting corn stalks into foam materials, especially foam materials that are lightweight, high-strength and have good thermal insulation properties that can meet the needs of industrial applications.

[0004] Therefore, developing a foam material with excellent performance using corn straw as raw material through innovative technology has important practical value and social significance. Summary of the invention

[0005] In view of the deficiencies in the prior art and the need for agricultural waste treatment and resource utilization, the present invention provides a foam material based on corn stalks, and a preparation method and application thereof. The present invention can transform corn stalks into a foam material with a porous structure through specific chemical and physical process treatment. The foam material of the present invention has light weight, high strength and good thermal insulation performance, and can be applied to the fields of thermal insulation, heat preservation, packaging, filling materials, etc.; the present invention can effectively utilize waste from agricultural production, reduce environmental pollution, and provide new environmentally friendly materials for the industrial field; these materials not only increase the added value of agricultural by-products, but also broaden their application range in multiple fields such as construction, packaging, and filling materials.

[0006] The technical solution of the present invention is as follows:

[0007] A foam material based on corn stalks is prepared by comprising the following raw materials in parts by weight: 2 to 30 parts of corn stalks, 0.5 to 5 parts of a foam stabilizer, 0.01 to 2 parts of a foaming agent, 0.1 to 2 parts of a flocculant, and 50 to 150 parts of deionized water.

[0008] Preferably according to the present invention, the corn straw-based foam material is prepared by comprising the following raw materials in parts by weight: 5 to 15 parts of corn straw, 2 to 4 parts of foam stabilizer, 0.01 to 0.10 parts of foaming agent, 0.1 to 0.3 parts of flocculant, and 100 to 150 parts of deionized water.

[0009] Preferably, the corn straw-based foam material is prepared by including the following raw materials in parts by weight: 10 parts of corn straw, 2.5-3.25 parts of foam stabilizer, 0.05-0.07 parts of foaming agent, 0.15-0.2 parts of flocculant, and 110-130 parts of deionized water.

[0010] Further preferably, the corn straw-based foam material is prepared by including the following raw materials in parts by weight: 10 parts of corn straw, 2.5-3.25 parts of foam stabilizer, 0.05-0.07 parts of foaming agent, 0.15 parts of flocculant, and 120 parts of deionized water.

[0011] Most preferably, the corn straw-based foam material is prepared by including the following raw materials in parts by weight: 10 parts of corn straw, 3.25 parts of foam stabilizer, 0.07 parts of foaming agent, 0.15 parts of flocculant, and 120 parts of deionized water.

[0012] Preferably according to the present invention, the foam stabilizer is one or a combination of two or more of polyvinyl alcohol (PVA), calcium stearate, starch or alkyl alcohol amide; preferably, the foam stabilizer is a combination of polyvinyl alcohol (PVA) and calcium stearate; the mass ratio of polyvinyl alcohol to calcium stearate is 1-1.6:1.

[0013] Preferably according to the present invention, the foaming agent is one or a combination of two or more of sodium dodecyl sulfate (SDS), sodium α-olefin sulfonate or hydrogen peroxide (hydrogen peroxide).

[0014] Preferably according to the present invention, the flocculant is one or a combination of two or more of polyacrylamide, lignin sulfonate, polyaluminium chloride or lithium carbonate.

[0015] The method for preparing the above-mentioned corn straw-based foam material comprises the following steps:

[0016] (1) Soaking corn stalks in deionized water to remove dust and impurities; then grinding and balancing the water content to obtain stalk slurry;

[0017] (2) adding a foam stabilizer to the straw slurry and stirring it thoroughly to disperse it evenly; adding a foaming agent and stirring it to foam; adding a flocculant and stirring it to promote foaming and forming; adding deionized water and stirring it thoroughly; and then drying it to obtain a corn straw-based foam material.

[0018] According to the preferred embodiment of the present invention, in step (1), the soaking temperature is 45-55°C, the soaking time is 10-12 hours, and the material is fully moistened by soaking. The amount of water used for soaking is only enough to immerse the straw.

[0019] Preferably, according to the present invention, in step (1), the refining is mechanical refining, and a disc refiner is used for refining; the refining is carried out in sequence at disc refiner gaps of 0.5 mm, 0.3 mm, and 0.1 mm, respectively, the refining time at each gap is 20-25 min, and the refining environment temperature is room temperature.

[0020] According to the present invention, in step (1), balancing the moisture content refers to adding deionized water to the pulp obtained by refining to obtain a straw pulp of a specific concentration.

[0021] Preferably according to the present invention, in step (1), the water content of the straw slurry is 70-80wt%.

[0022] Preferably according to the present invention, in step (2), before adding the foam stabilizer to the straw slurry, the method further comprises the step of stirring and dispersing the straw slurry; the stirring rate is 200-400 r / min, the stirring time is 20-40 min, and the stirring temperature is room temperature.

[0023] Preferably, in step (2), after adding the foam stabilizer, the stirring temperature is room temperature, the stirring time is 5-15 min, the stirring rate is 300-400 r / min, and the stirring is performed until the system becomes a paste.

[0024] Preferably, according to the present invention, in step (2), the stirring temperature after adding the foaming agent is room temperature, the stirring rate is 400-600 r / min, and the stirring time is 10-25 min.

[0025] Preferably, according to the present invention, in step (2), the stirring temperature after adding the flocculant is room temperature, the stirring time is 5-10 min, and the stirring rate is 400-600 r / min.

[0026] Preferably, according to the present invention, in step (2), the stirring temperature after adding deionized water is room temperature, the stirring rate is 400-600 r / min, and the stirring time is 5-30 min, until the volume of the entire foaming system no longer changes.

[0027] Preferably according to the present invention, in step (2), the drying is freeze-drying.

[0028] The above-mentioned corn straw-based foam material is applied to thermal insulation material, heat preservation material or thermal insulation foam cushioning filling material.

[0029] The technical features and beneficial effects of the present invention are as follows:

[0030] 1. The raw materials of the corn stalk-based foam material of the present invention are cheap and easy to obtain, and the preparation process is simple, efficient and clean, and no complicated experimental operation is required. In the preparation process of the present invention, corn stalks are first used as raw materials, and the stalks are treated by soaking at a specific temperature, and the treatment plays an auxiliary role in the subsequent pulping. Subsequently, a foam stabilizer is added to the system, and after the foam stabilizer penetrates into the interior of the fiber, a preliminary foam base is formed by compounding. The foaming agent added is foamed under the action of the foam stabilizer to generate a mixture with a certain pore structure, which lays the foundation for the lightweight and thermal insulation properties of the foam material. Then the interaction between the flocculant and the foaming agent, as well as the appropriate amount of water content, jointly promote the final formation of the foam material, ensuring the lightweight and efficient thermal insulation properties of the material. Through the above-mentioned process steps, the corn stalk-based foam material finally prepared has the characteristics of low density and high porosity, while ensuring the thermal insulation performance and structural stability of the material.

[0031] 2. The foaming agent used in the present invention plays a vital role in the process of preparing corn straw-based foam materials. On the one hand, it significantly improves the foaming efficiency, effectively reduces the liquid interfacial tension, has stable structural properties, and is applicable to a wide range of temperature, humidity and pH, ensuring the rapid formation and structural stability of the foam material. On the other hand, the foaming agent used in the present invention is non-toxic, safe and environmentally friendly; no toxic gas is generated during the foaming process. In actual industrial production, this process not only improves production efficiency, but also reduces the dangers that may arise in large-scale industrial production processes, and effectively reduces production costs.

[0032] The specific type and ratio of the foaming agent in the present invention are specially designed for the corn straw raw material system, ensuring the efficient reaction and the excellent performance of the foam material. If the type or ratio of the foaming agent is changed, the lightweight and efficient thermal insulation foam material described in the present invention cannot be obtained, and the environmental protection and performance advantages expected by the present invention cannot be achieved. Therefore, the selection and use of the foaming agent is one of the key factors in achieving the technical characteristics and beneficial effects of the present invention.

[0033] 3. The raw materials of the present invention are carefully proportioned and coordinated as a whole, and a small amount of flocculant is selected to assist foaming. This foaming method using composite additives can achieve the expected foaming effect with less foaming agent and flocculant, improve the foaming efficiency of production and make it easier to form. By accurately controlling the amount of reagents used in the foam formation process, it can avoid poor effects due to insufficient dosage and prevent unnecessary production costs due to excessive use, thereby achieving dual optimization of cost-effectiveness and production efficiency.

[0034] 4. The raw material composition of the corn stalk-based foam material of the present invention is specific, ensuring the unique performance and effect of the material. Only through the specific raw material types and precise proportions of the present invention can the characteristics of the foam material such as light weight and high-efficiency heat insulation be achieved. For example, corn stalks are used as the main raw material, and their unique chemical structure and physical properties are the key to achieving low density and high porosity of foam materials. In addition, the addition of organic foam stabilizers not only provides the necessary chemical cross-linking for the material, improves the mechanical strength of the molding, but also helps to ensure its heat insulation performance. Suitable deionized water is crucial to achieving the excellent performance of the material; insufficient dosage may lead to foaming failure, while excessive dosage may cause excessive foaming and reduce the mechanical properties and stability of the foam material. Only when the raw materials interact with each other under precise proportions can a foam material with the desired pore structure be effectively formed. As a whole, the raw material composition of the present invention achieves the expected effect of the foam material through the synergistic effect of each raw material.

[0035] 5. In the method for preparing the corn straw-based foam material of the present invention, the foam stabilizer is added before the foaming agent. This order is crucial to ensure the successful preparation and excellent performance of the material. If this order is changed, the lightweight and efficient thermal insulation foam material described in the present invention cannot be obtained, and the expected physical properties and environmental characteristics cannot be achieved. In each reaction step, the order of adding reagents and raw materials, as well as the types and ratios of foaming agents, foam stabilizers, and flocculants are all key factors affecting the quality of the final foam material.

[0036] Only by adding the foam stabilizer first can the raw materials such as straw pulp be wrapped in the organic system of the foam stabilizer in the subsequent foaming reaction, so that the slurry can be dispersed more evenly to form a uniform and stable foam structure. If the order of this step is reversed, the uniform dispersion of the slurry and the added reagent will not be effectively achieved, thereby affecting the final performance of the foam material. Therefore, the preparation method of the present invention as a whole, the precise coordination of each step and condition is the basis for achieving the excellent effect of the foam material. The foam material prepared by this method can not only provide a new way for the reuse of agricultural waste, but also has a wide range of application prospects due to its excellent physical properties and environmental protection characteristics.

[0037] 6. The foam material of the present invention has stable pores, is lightweight, and exhibits good mechanical stiffness (with a high Young's modulus) and thermal insulation, and can maintain its performance under various environmental conditions. This has important application value in many fields such as building insulation and cold chain logistics, and also makes it widely used in the field of life as an excellent thermal insulation buffer filling material. The thermal insulation properties of the foam material are particularly outstanding. When the foam is made of a variety of different raw material ratios, its thermal conductivity is as low as 0.0312W / (m·K); according to national standards, when the average temperature is not higher than 350°C, materials with a thermal conductivity of no more than 0.12W / (m·K) can be called thermal insulation materials; and materials with a thermal conductivity of less than 0.05W / (m·K) are considered to be high-efficiency thermal insulation materials; this shows that the foam material of the present invention can meet the stringent conditions of being an excellent thermal insulation material.

[0038] In addition, the foam material of the present invention also exhibits very good mechanical rigidity. When the foam is made of several different raw material ratios, the obtained foam material has a high Young's modulus. The foam material made under the preferred ratio of the present invention has a very high rebound cushioning performance and a relatively strong structure. Therefore, the foam material of the present invention can be used as an excellent thermal insulation cushioning filling material and has great application potential in multiple fields of life.

[0039] And, due to the natural properties of corn straw, this foam material is biodegradable, which helps reduce environmental pollution and promotes sustainable development, making it an ideal packaging or insulation material.

[0040] At the same time, the present invention effectively utilizes waste from agricultural production, reduces environmental pollution, and provides new environmentally friendly materials for the industrial field; it increases the added value of agricultural by-products, and provides innovative solutions for the environmental protection treatment and resource utilization of agricultural waste, which has important social and economic significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 A top view (a) and a front view (b) of the foam material prepared in Example 1;

[0042] Figure 2 This is a test graph of thermal conductivity of the foam material prepared in Example 1;

[0043] Figure 3 This is the stress-strain curve of the foam material prepared in Example 1. DETAILED DESCRIPTION

[0044] The present invention is further described below with reference to specific embodiments, but is not limited thereto.

[0045] Meanwhile, the experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0046] Example 1

[0047] A corn stalk-based foam material is prepared by including the following raw materials in parts by weight: 10.0 g of corn stalk, 2.0 g of (foam stabilizer) polyvinyl alcohol (polyvinyl alcohol 1750), 1.25 g of (foam stabilizer) calcium stearate, 0.07 g of a foaming agent (sodium α-olefin sulfonate), 0.15 g of a flocculant (lithium carbonate), and 120.0 g of deionized water.

[0048] The specific steps of the method for preparing the above-mentioned corn straw-based foam material are as follows.

[0049] Step 1: Raw material preparation

[0050] Cut all the prepared corn stalks into short segments of about 5cm-6cm, prepare 1kg of corn stalks at a time and immerse them in warm water for 12 hours at a water temperature of 50℃. Soak to remove some dust and impurities, fully moisten the material, and prepare for mechanical refining.

[0051] Step 2: Refining

[0052] The raw material obtained in step (i) was refined at room temperature using a continuous high-concentration disc refiner at disc gaps of 0.5 mm, 0.3 mm, and 0.1 mm, respectively, for 25 min at each disc gap. Deionized water was added to balance the moisture content to obtain a straw slurry with a moisture content of 75 wt%.

[0053] Step (3) Foaming reaction

[0054] 40 g of the straw slurry obtained in step (ii) (including 10 g of corn stalks) was added to a beaker and stirred at room temperature for 30 min at a speed of 300 r / min to evenly disperse the slurry; a foam stabilizer was added, and 1.25 g of powdered calcium stearate was first added to the foam stabilizer, and the foam stabilizer was stirred at room temperature for 5 min at a speed of 400 r / min to be fully mixed with the fiber slurry, and then a polyvinyl alcohol aqueous solution (containing 2.0 g of polyvinyl alcohol and a solvent of 50 g of deionized water) was added, and the foaming agent was stirred at room temperature for 10 min at a speed of 400 r / min until it became a paste; 0.07 g of sodium α-olefin sulfonate was added as a foaming agent, and the foaming agent was rapidly stirred at room temperature at 500 r / min for 20 min; then 0.15 g of lithium carbonate was added as a flocculant, and the foaming agent was stirred at room temperature at 500 r / min for 10 min to promote foaming and molding; finally, 40 g of deionized water was added for quantitative determination, and the total moisture content was 120 g. The mixture was stirred at room temperature at a speed of 500 r / min for 20 min until the volume of the entire foaming system stopped changing. The foaming volume was recorded as 531 mL, and the foaming was terminated.

[0055] Step 4: Foam molding

[0056] The composite straw slurry foam obtained in step (iii) was quickly transferred to a metal cylindrical container (diameter 50 mm, height 40 mm) with a movable bottom, and the volume before drying was recorded; the container containing the foam was completely frozen and placed in a vacuum dryer for drying for 60 h. After drying was completed, the container was taken out; the foam was taken out from the container to obtain a foam sample, and the foam volume after drying was recorded.

[0057] The top view (a) and front view (b) of the foam material prepared in this embodiment are as follows Figure 1 As shown in the figure, it can be seen that the prepared foam material has regular molding and high porosity.

[0058] The thermal conductivity test graph of the foam material prepared in this embodiment is as follows Figure 2 As shown in the figure, it can be seen that after the hot wire method test, the foam material has a large temperature difference within the test time and a small thermal conductivity, and is suitable for the preparation of thermal insulation materials.

[0059] The stress-strain curve of the foam material prepared in this example is as follows: Figure 3 As shown, three samples were tested in parallel. It can be seen from the figure that the foam material has a smaller deformation under a pressure of 0.02MPa, which means that the foam material has a higher stiffness, that is, a higher Young's modulus value.

[0060] Example 2

[0061] A corn stalk-based foam material is prepared by including the following raw materials in parts by weight: 10.0 g of corn stalk, 1.25 g of (foam stabilizer) polyvinyl alcohol (polyvinyl alcohol 1750), 1.25 g of (foam stabilizer) calcium stearate, 0.06 g of a foaming agent (sodium α-olefin sulfonate), 0.15 g of a flocculant (lithium carbonate), and 120.0 g of deionized water.

[0062] In the method for preparing the above-mentioned corn straw-based foam material, the raw material amounts are the same as above, and the remaining steps and conditions are the same as in Example 1.

[0063] Example 3

[0064] A corn stalk-based foam material is prepared by including the following raw materials in parts by weight: 10.0 g of corn stalk, 1.25 g of (foam stabilizer) polyvinyl alcohol (polyvinyl alcohol 1750), 1.25 g of (foam stabilizer) calcium stearate, 0.06 g of foaming agent (sodium α-olefin sulfonate), 0.15 g of flocculant (lithium carbonate), and 115.0 g of deionized water.

[0065] The method for preparing the above-mentioned corn straw-based foam material comprises the following steps:

[0066] Steps (1) and (2) are the same as in Example 1;

[0067] Step (3) Foaming reaction

[0068] 40 g of the straw slurry obtained in step (ii) (including 10 g of corn stalks) was added to a beaker and stirred at room temperature for 30 min at a speed of 300 r / min to evenly disperse the slurry; a foam stabilizer was added, and 1.25 g of powdered calcium stearate was first added to the foam stabilizer, and the foam stabilizer was stirred at room temperature for 5 min at a speed of 400 r / min to be fully mixed with the fiber slurry, and then a polyvinyl alcohol aqueous solution (containing 1.25 g of polyvinyl alcohol and a solvent of 50 g of deionized water) was added, and the foaming agent was stirred at room temperature for 10 min at a speed of 400 r / min until it became a paste; 0.06 g of sodium α-olefin sulfonate was added as a foaming agent, and the foaming agent was rapidly stirred at room temperature at 500 r / min for 20 min; then 0.15 g of lithium carbonate was added as a flocculant, and the mixture was stirred at room temperature at 500 r / min for 10 min to promote foaming and molding; finally, 35 g of deionized water was added for quantitative determination, and the total moisture content was 115 g. The mixture was stirred at room temperature at a speed of 500 r / min for 20 min until the volume of the entire foaming system no longer changed, and the foaming was terminated.

[0069] Step (iv) is the same as in Example 1.

[0070] Example 4

[0071] A corn stalk-based foam material is prepared by including the following raw materials in parts by weight: 10.0 g of corn stalk, 1.25 g of (foam stabilizer) polyvinyl alcohol (polyvinyl alcohol 1750), 1.25 g of (foam stabilizer) calcium stearate, 0.07 g of a foaming agent (sodium α-olefin sulfonate), 0.20 g of a flocculant (lithium carbonate), and 110.0 g of deionized water.

[0072] The method for preparing the above-mentioned corn straw-based foam material comprises the following steps:

[0073] Steps (1) and (2) are the same as in Example 1;

[0074] Step (3) Foaming reaction

[0075] 40 g of the straw slurry obtained in step (ii) (including 10 g of corn stalks) was added to a beaker and stirred at room temperature for 30 min at a speed of 300 r / min to evenly disperse the slurry; a foam stabilizer was added, and 1.25 g of powdered calcium stearate was first added to the foam stabilizer, and the foam stabilizer was stirred at room temperature for 5 min at a speed of 400 r / min to be fully mixed with the fiber slurry, and then a polyvinyl alcohol aqueous solution (containing 1.25 g of polyvinyl alcohol and a solvent of 50 g of deionized water) was added, and the foaming agent was stirred at room temperature for 10 min at a speed of 400 r / min until it became a paste; 0.07 g of sodium α-olefin sulfonate was added as a foaming agent, and the foaming agent was rapidly stirred at room temperature at 500 r / min for 20 min; then 0.2 g of lithium carbonate was added as a flocculant, and the foaming agent was stirred at room temperature at 500 r / min for 10 min to promote foaming and molding; finally, 30 g of deionized water was added for quantitative determination, and the total moisture content was 110 g. The mixture was stirred at room temperature at a speed of 500 r / min for 20 min until the volume of the entire foaming system no longer changed, and the foaming was terminated.

[0076] Step (iv) is the same as in Example 1.

[0077] Example 5

[0078] A corn stalk-based foam material is prepared by including the following raw materials in parts by weight: 10.0 g of corn stalk, 1.25 g of (foam stabilizer) polyvinyl alcohol (polyvinyl alcohol 1750), 1.25 g of (foam stabilizer) calcium stearate, 0.05 g of a foaming agent (sodium α-olefin sulfonate), 0.15 g of a flocculant (lithium carbonate), and 120.0 g of deionized water.

[0079] In the method for preparing the above-mentioned corn straw-based foam material, the amount of raw materials used is the same as above, and the remaining steps and conditions are the same as Example 2.

[0080] Example 6

[0081] A corn stalk-based foam material is prepared by including the following raw materials in parts by weight: 10.0 g of corn stalk, 1.50 g of (foam stabilizer) polyvinyl alcohol (polyvinyl alcohol 1750), 1.25 g of (foam stabilizer) calcium stearate, 0.06 g of foaming agent (sodium α-olefin sulfonate), 0.15 g of flocculant (lithium carbonate), and 110.0 g of deionized water.

[0082] The method for preparing the above-mentioned corn straw-based foam material comprises the following steps:

[0083] Steps (1) and (2) are the same as in Example 1;

[0084] Step (3) Foaming reaction

[0085] 40 g of the straw slurry obtained in step (ii) (including 10 g of corn stalks) was added to a beaker and stirred at room temperature for 30 min at a speed of 300 r / min to evenly disperse the slurry; a foam stabilizer was added, and 1.25 g of powdered calcium stearate was first added to the foam stabilizer, and the foam stabilizer was stirred at room temperature for 5 min at a speed of 400 r / min to be fully mixed with the fiber slurry, and then a polyvinyl alcohol aqueous solution (containing 1.5 g of polyvinyl alcohol and a solvent of 50 g of deionized water) was added, and the foaming agent was stirred at room temperature for 10 min at a speed of 400 r / min until it became a paste; 0.06 g of sodium α-olefin sulfonate was added as a foaming agent, and the foaming agent was rapidly stirred at room temperature at 500 r / min for 20 min; then 0.15 g of lithium carbonate was added as a flocculant, and the foaming agent was stirred at room temperature at 500 r / min for 10 min to promote foaming and molding; finally, 30 g of deionized water was added for quantitative determination, and the total moisture content was 110 g. The mixture was stirred at room temperature at a speed of 500 r / min for 20 min until the volume of the entire foaming system no longer changed, and the foaming was terminated.

[0086] Step (iv) is the same as in Example 1.

[0087] Example 7

[0088] A corn stalk-based foam material is prepared by including the following raw materials in parts by weight: 10.0 g of corn stalk, 2.00 g of (foam stabilizer) polyvinyl alcohol (polyvinyl alcohol 1750), 1.25 g of (foam stabilizer) calcium stearate, 0.07 g of foaming agent (sodium α-olefin sulfonate), 0.15 g of flocculant (lithium carbonate), and 130.0 g of deionized water.

[0089] The method for preparing the above-mentioned corn straw-based foam material comprises the following steps:

[0090] Steps (1) and (2) are the same as in Example 1;

[0091] Step (3) Foaming reaction

[0092] 40 g of the straw slurry obtained in step (ii) (including 10 g of corn stalks) was added to a beaker and stirred at room temperature for 30 min at a speed of 300 r / min to evenly disperse the slurry; a foam stabilizer was added, and 1.25 g of powdered calcium stearate was first added to the foam stabilizer, and the foam stabilizer was stirred at room temperature for 5 min at a speed of 400 r / min to be fully mixed with the fiber slurry, and then a polyvinyl alcohol aqueous solution (containing 2 g of polyvinyl alcohol, and the solvent was 50 g of deionized water) was added, and the foaming agent was stirred at room temperature for 10 min at a speed of 400 r / min until it became a paste; 0.07 g of sodium α-olefin sulfonate was added as a foaming agent, and the foaming agent was rapidly stirred at room temperature at 500 r / min for 20 min; then 0.15 g of lithium carbonate was added as a flocculant, and the foaming agent was stirred at room temperature at 500 r / min for 10 min to promote foaming and molding; finally, 50 g of deionized water was added for quantitative determination, and the total moisture content was 130 g. The mixture was stirred at room temperature at a speed of 500 r / min for 20 min until the volume of the entire foaming system no longer changed, and the foaming was terminated.

[0093] Step (iv) is the same as in Example 1.

[0094] Example 8

[0095] A corn stalk-based foam material is prepared by including the following raw materials in parts by weight: 10.0 g of corn stalk, 2.00 g of (foam stabilizer) polyvinyl alcohol (polyvinyl alcohol 1750), 1.25 g of (foam stabilizer) calcium stearate, 0.06 g of foaming agent (sodium α-olefin sulfonate), 0.15 g of flocculant (lithium carbonate), and 120.0 g of deionized water.

[0096] In the method for preparing the above-mentioned corn straw-based foam material, the raw material amounts are the same as above, and the remaining steps and conditions are the same as in Example 1.

[0097] Example 9

[0098] A corn straw-based foam material, as described in Example 1, except that no polyvinyl alcohol (PVA) is added; other raw material compositions are the same as in Example 1.

[0099] The preparation method of the above-mentioned corn straw-based foam material is as described in Example 1, except that no polyvinyl alcohol (PVA) is added, that is, the polyvinyl alcohol aqueous solution is replaced by 50 g of deionized water; the other steps and conditions are the same as in Example 1.

[0100] Example 10

[0101] A foam material based on corn stalks, as described in Example 1, except that calcium stearate is not added; other raw material compositions are the same as in Example 1.

[0102] The method for preparing the above-mentioned corn straw-based foam material is as described in Example 1, except that calcium stearate is not added; the other steps and conditions are the same as in Example 1.

[0103] Embodiment 11

[0104] A foam material based on corn stalks, as described in Example 1, except that the foaming agent is changed to 30wt% hydrogen peroxide; the other raw material compositions are the same as those in Example 1.

[0105] The method for preparing the above-mentioned corn straw-based foam material is as described in Example 1, except that the foaming agent is changed to 30 wt % hydrogen peroxide; the other steps and conditions are the same as in Example 1.

[0106] Example 12

[0107] A foam material based on corn stalks, as described in Example 1, except that the foaming agent is changed to sodium dodecyl sulfate (SDS); the other raw material compositions are the same as in Example 1.

[0108] The method for preparing the above-mentioned corn straw-based foam material is as described in Example 1, except that the foaming agent is changed to sodium dodecyl sulfate (SDS); the other steps and conditions are the same as in Example 1.

[0109] Embodiment 13

[0110] A corn straw-based foam material, as described in Example 1, except that the foaming agent is changed to a combination of sodium dodecyl sulfate (SDS) (0.03 g) and sodium α-olefin sulfonate (0.04 g); the other raw material compositions are the same as in Example 1.

[0111] The method for preparing the above-mentioned corn straw-based foam material is as described in Example 1, except that the foaming agent is changed to a combination of sodium dodecyl sulfate (SDS) and sodium α-olefin sulfonate; the other steps and conditions are the same as in Example 1.

[0112] Embodiment 14

[0113] A corn straw-based foam material, as described in Example 1, except that lithium carbonate is replaced by polyacrylamide; other raw material compositions are the same as in Example 1.

[0114] The method for preparing the above-mentioned corn straw-based foam material is as described in Example 1, except that lithium carbonate is replaced by polyacrylamide; the other steps and conditions are the same as in Example 1.

[0115] Comparative Example 1

[0116] A foam material, as described in Example 1, except that polyvinyl alcohol and calcium stearate are not added; other raw material compositions are the same as those in Example 1.

[0117] The preparation method of the above foam is as described in Example 1, except that polyvinyl alcohol and calcium stearate are not added; the other steps and conditions are the same as in Example 1.

[0118] Comparative Example 2

[0119] A foam material, the raw material composition is the same as that of embodiment 1.

[0120] The method for preparing the foam is as described in Example 1, except that the order of adding the foam stabilizer and the foaming agent is changed;

[0121] The details are as follows:

[0122] Steps (i) and (ii) are the same as in Example 1;

[0123] Step (3) Foaming reaction

[0124] 40 g of the straw slurry obtained in step (ii) (including 10 g of corn stalks) was added to a beaker, and stirred at room temperature for 30 min at a speed of 300 r / min to evenly disperse the slurry; 0.07 g of sodium α-olefin sulfonate as a foaming agent was added, and the mixture was rapidly stirred and foamed at room temperature at 500 r / min for 20 min; a foam stabilizer was added, and first 1.25 g of powdered calcium stearate was added to the foam stabilizer, and the mixture was stirred at room temperature at a speed of 400 r / min for 5 min, and then a polyvinyl alcohol aqueous solution (containing 2.0 g of polyvinyl alcohol and a solvent of 50 g of deionized water) was added, and the mixture was stirred at room temperature at a speed of 400 r / min for 10 min; then 0.15 g of lithium carbonate as a flocculant was added, and the mixture was stirred at room temperature at a speed of 500 r / min for 10 min to promote foaming and molding; finally, 40 g of deionized water was added for quantitative determination, and the total moisture content was 120 g. The mixture was stirred at room temperature at a speed of 500 r / min for 20 min until the volume of the entire foaming system no longer changed. The foaming volume was recorded as 503 mL, and the foaming was terminated.

[0125] Step (iv) is the same as in Example 1.

[0126] Comparative Example 3

[0127] A foam material, as described in Example 1, except that lithium carbonate is not added; other raw material compositions are the same as those in Example 1.

[0128] The method for preparing the foam is as described in Example 1, except that lithium carbonate is not added; the other steps and conditions are the same as in Example 1.

[0129] Finally, the foaming failed and no foam material was obtained. It can be seen that lithium carbonate can promote foaming as a flocculant. Without the addition of lithium carbonate, the foaming process will be more difficult.

[0130] Test example

[0131] The foamed materials prepared in the examples and comparative examples were tested for foaming volume, density, Young's modulus, and thermal conductivity. The test results are shown in Table 1.

[0132] Table 1

[0133]

[0134]

[0135] From the test results in Table 1, we can compare and analyze the Young's modulus and thermal conductivity of the foam materials in the examples. Young's modulus is an indicator of the elasticity of the material, while the thermal conductivity reflects the thermal conductivity of the material. These two parameters are crucial for evaluating the performance of the foam material.

[0136] First, in all successful examples, the Young's modulus ranges from 0.012 MPa to 0.166 MPa. The Young's modulus of Example 1 is 0.162 MPa, that of Example 11 is 0.152 MPa, that of Example 12 is 0.166 MPa, that of Example 13 is 0.163 MPa, and that of Example 14 is 0.156 MPa. This indicates that the foam materials of these examples have good elasticity.

[0137] Next, the thermal conductivity ranges from 0.0312 W / (m·K) to 0.0453 W / (m·K). The thermal conductivity of Example 1 is 0.0336 W / (m·K), Example 3 is 0.0312 W / (m·K), Example 5 is 0.0321 W / (m·K), Example 9 is 0.0331 W / (m·K), Example 10 is 0.0338 W / (m·K), and Example 13 is 0.0354 W / (m·K). These values ​​show that the foam materials of these examples have good thermal insulation properties.

[0138] Therefore, the foam material obtained by the present invention has the advantages of light weight, high elasticity and high strength, and at the same time, the characteristic of low thermal conductivity makes it have good thermal insulation performance.

[0139] In the above embodiments, by comprehensively comparing the performance parameters such as Young's modulus and thermal conductivity of the materials, the effects of Embodiment 1 and Embodiment 13 are relatively good. Preferably, Embodiment 1 has the best overall effect.

[0140] 1. The foam materials of Examples 1 and 13 have better elasticity and thermal insulation properties.

[0141] 2. The Young's modulus and thermal conductivity of Example 1 are both at a relatively high level, indicating that it has good thermal insulation performance while maintaining good elasticity.

[0142] Therefore, according to the above analysis, Example 1 has the best overall effect, which is due to its good balance between Young's modulus and thermal conductivity. This balance is very important for the practical application of foam materials because it is most likely to affect the durability and thermal management capabilities of the material.

Claims

1. A foam material based on corn stalks, characterized in that: The preparation method comprises the following raw materials in parts by weight: 2 to 30 parts of corn stalks, 0.5 to 5 parts of foam stabilizer, 0.01 to 2 parts of foaming agent, 0.1 to 2 parts of flocculant, and 50 to 150 parts of deionized water.

2. The corn straw-based foam material according to claim 1, characterized in that: The corn stalk-based foam material is prepared by including the following raw materials in parts by weight: 5 to 15 parts of corn stalks, 2 to 4 parts of foam stabilizers, 0.01 to 0.10 parts of foaming agents, 0.1 to 0.3 parts of flocculants, and 100 to 150 parts of deionized water.

3. The corn straw-based foam material according to claim 2, characterized in that: The corn stalk-based foam material is prepared by including the following raw materials in parts by weight: 10 parts of corn stalks, 2.5-3.25 parts of foam stabilizer, 0.05-0.07 parts of foaming agent, 0.15-0.2 parts of flocculant, and 110-130 parts of deionized water.

4. The corn straw-based foam material according to claim 1, characterized in that: The foam stabilizer is one or a combination of two or more of polyvinyl alcohol (PVA), calcium stearate, starch or alkyl alcohol amide; preferably, the foam stabilizer is a combination of polyvinyl alcohol (PVA) and calcium stearate; the mass ratio of polyvinyl alcohol to calcium stearate is 1-1.6:

1.

5. The corn straw-based foam material according to claim 1, characterized in that: The foaming agent is one or a combination of two or more of sodium dodecyl sulfate (SDS), sodium α-olefin sulfonate or hydrogen peroxide (hydrogen peroxide).

6. The corn straw-based foam material according to claim 1, characterized in that: The flocculant is one or a combination of two or more of polyacrylamide, lignin sulfonate, polyaluminium chloride or lithium carbonate.

7. The method for preparing a corn straw-based foam material according to any one of claims 1 to 6, comprising the steps of: (1) Soaking corn stalks in deionized water to remove dust and impurities; then grinding and balancing the water content to obtain stalk slurry; (2) adding a foam stabilizer to the straw slurry and stirring it thoroughly to disperse it evenly; adding a foaming agent and stirring it to foam; adding a flocculant and stirring it to promote foaming and forming; adding deionized water and stirring it thoroughly; and then drying it to obtain a corn straw-based foam material.

8. The method for preparing the corn straw-based foam material according to claim 7, characterized in that: In step (1), one or more of the following conditions are included: i. The soaking temperature is 45-55℃, and the soaking time is 10-12h. The soaking is to fully moisten the material; ii. The pulping is mechanically refined by using a disc refiner; the pulping is performed in sequence at disc refining gaps of 0.5 mm, 0.3 mm, and 0.1 mm, respectively, the refining time at each gap is 20-25 minutes, and the refining environment temperature is room temperature; iii. The water content of the straw slurry is 70-80wt%.

9. The method for preparing the corn straw-based foam material according to claim 7, characterized in that: In step (2), one or more of the following conditions are included: i. Before adding the foam stabilizer to the straw slurry, the method further comprises the step of stirring and dispersing the straw slurry; the stirring rate is 200-400 r / min, the stirring time is 20-40 min, and the stirring temperature is room temperature; ii. After adding the foam stabilizer, the stirring temperature is room temperature, the stirring time is 5-15min, the stirring rate is 300-400r / min, and the system is stirred until it becomes a paste; iii. After adding the foaming agent, the stirring temperature is room temperature, the stirring rate is 400-600r / min, and the stirring time is 10-25min; iv. After adding the flocculant, the stirring temperature is room temperature, the stirring time is 5-10 min, and the stirring rate is 400-600 r / min; v. After adding deionized water, the stirring temperature is room temperature, the stirring rate is 400-600r / min, and the stirring time is 5-30min, until the volume of the entire foaming system no longer changes; vi. Drying is freeze drying.

10. The use of the corn straw-based foam material as claimed in any one of claims 1 to 6, wherein the characteristic function is that the foam material is used as a thermal insulation material, a heat preservation material or a thermal insulation foam cushioning filling material.

Citation Information

Patent Citations

  • Super light polymer foamed concrete and preparation method thereof

    CN102424551A

  • Preparation method of modified common silicate cement based foam insulating plate and special assistant

    CN103183487A

  • Plant fiber porous composite material

    CN103772749A

  • Method for preparing non-bearing heat preservation material by adopting corn stalks as raw materials

    CN106220228A

  • Starch / polyvinyl alcohol composite foaming material composition and preparation method thereof

    CN109135311A