Inorganic anticorrosive coating with double functions of chloride ion fixation and damage self-repairing
By combining the interaction between hydroxyapatite and phosphate phase in the inorganic anticorrosion coating, a stable film-forming substance and releasing the phosphate phase under specific conditions, the chloride ion erosion problem of reinforced concrete structures in the marine environment is solved, and achievable High durability and self-repairing effect of damage, significantly improving the corrosion resistance and bonding strength of the structure.
Patent Information
- Application Number
- CN202310597804.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-25
AI Technical Summary
The existing reinforced concrete structures are susceptible to chloride ions erosion and carbonization in the marine environment, resulting in corrosion, resulting in damage to concrete structures. The existing inorganic anticorrosion coatings lack self-repairing ability, which affects the structure life and safety.
Develop an inorganic anticorrosion coating containing hydroxyapatite, phosphate and fusion phase to form a stable film-forming substance through the interaction between the matrix and the phosphate phase, and release the phosphate phase under specific conditions to fix chloride ions And form a protective precipitation film to achieve self-healing of damage.
The coating has no change in the 8000-hour xenon lamp aging test, and has high hardness. It can effectively fix chloride ions and form a protective film after damage, which significantly improves the corrosion resistance of the steel bars and the bonding strength of the structure.
Smart Images

Figure CN119019869A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of corrosion protection of reinforced concrete structures, and in particular relates to an inorganic anti-corrosion coating for steel bar corrosion protection, which has the dual functions of chloride ion fixation and damage self-repair. Background Art
[0002] The construction of marine islands and reefs is of great significance to improving the navy's far sea combat capability. The long-term safe service of military infrastructure on islands and reefs is the backup basic guarantee for the safety of life and equipment of military personnel on the islands. At present, the construction of military docks, island and reef infrastructure, etc. is mainly based on concrete structures. However, chloride ion erosion and concrete carbonization in the marine environment will cause corrosion of steel bars in concrete structures, causing damage to concrete structures, and seriously affecting the service life and safety of military infrastructure.
[0003] Steel bar anti-corrosion coating can effectively improve the corrosion resistance of steel bars. Generally, intact coatings have good anti-corrosion effects, but defects and damage will inevitably occur in the coating during construction and service, providing a penetration path for corrosive media, thereby seriously reducing the anti-corrosion performance of the coating. Damage self-repairing coatings can release curing agents or corrosion inhibitors when the coating is damaged, physically repair the coating or form a protective film, thereby reducing the corrosion of steel bars. However, most of the current damage self-repairing coatings are organic materials, which have the disadvantages of poor aging resistance and so on. In addition, the hardness of organic coatings is low, which will increase the bond slip between steel bars and concrete and reduce the bond strength. Although inorganic coatings have advantages in terms of material durability, mechanical strength, heat resistance, etc., they generally do not have damage self-repair capabilities. Therefore, how to develop an inorganic anti-corrosion coating with high durability, high mechanical strength, and self-repair when damaged has become an urgent problem to be solved in the development of long-life concrete structures. Summary of the invention
[0004] In order to overcome the deficiencies of the prior art, the present invention provides an inorganic anticorrosion coating with high durability, high hardness, and the dual functions of chloride ion fixation and damage self-repair.
[0005] The solution adopted by the present invention to solve its technical problem is: an inorganic anticorrosive coating with the dual functions of chloride ion fixation and damage self-repair, comprising the following components by weight: 30 to 70 parts of a matrix phase, 10 to 40 parts of a hydroxyapatite phase, 10 to 30 parts of a phosphate phase, and 10 to 20 parts of a flux phase; a portion of the phosphate phase can interact with the matrix phase to jointly constitute a basic film-forming material, forming a non-releasable phosphate phase that is not easily dissolved during the service of the coating; another portion of the phosphate phase is distributed in the basic film-forming material through a filling effect, and is dissolved under specific inducing conditions to form a releasable phosphate phase.
[0006] Furthermore, the matrix phase consists of three parts, the first part is any one of sodium borate and potassium borate or a combination of two, the second part is any one of sodium carbonate and potassium carbonate or a combination of two, and the third part is sodium silicate and calcium fluoride.
[0007] Furthermore, the hydroxyapatite phase is any one or a combination of two or more of hydroxy calcium apatite, hydroxy magnesium apatite, hydroxy sodium apatite, hydroxy potassium apatite and derivatives thereof.
[0008] The hydroxyapatite phase, the hydroxyapatite raw material passes through a 200-mesh sieve, the hydroxyapatite has sufficient stability, compatibility and chemical inertness in the matrix phase, can be evenly distributed in the coating and form a network structure, and is tightly combined with the matrix.
[0009] Furthermore, the phosphate phase is any one or a combination of two or more of sodium phosphate, potassium phosphate, zinc phosphate and magnesium phosphate.
[0010] Furthermore, the flux phase is any one or a combination of two or more of boron oxide, phosphorus pentoxide, bismuth oxide, and zinc oxide.
[0011] Furthermore, the coating has a thickness of 50 to 500 μm.
[0012] Furthermore, the coating is applied to the surface of the steel bar at a high temperature of 400 to 700°C.
[0013] An inorganic anticorrosive coating having the dual functions of chloride ion fixation and damage self-repair as described above, the coating is composed of pure inorganic materials, has no change in the xenon lamp aging test for 8000 hours, and has excellent durability. The coating has high hardness, and the Vickers hardness can reach 300-1000HV, which will be beneficial to the bonding between the coated steel bars and concrete, especially can improve the bonding stiffness in the small slip stage.
[0014] An inorganic anticorrosive coating having the dual functions of chloride ion fixation and damage self-repair as described above, the coating has the function of fixing chloride ions. In the early stage of concrete structure construction, the concrete pore solution is mainly saturated calcium hydroxide, with a pH of about 12 to 13.5. At this time, the coating can remain relatively stable in the concrete pore solution; as the chloride ions completely penetrate the concrete and reach the surface of the coating, the coating acts as a physical barrier to isolate the corrosive medium and the steel substrate; on the other hand, under the conditions of alkaline pore solution and chloride ions in the concrete, the uniform and network-distributed hydroxyapatite phase in the coating is activated, which reacts with chloride ions to form chloroapatite, which has the effect of fixing chloride ions, consumes corrosive chloride ions, and effectively inhibits the occurrence of steel corrosion.
[0015] An inorganic anticorrosive coating having the dual functions of chloride ion fixation and damage self-repair as described above, the coating has the function of forming a damage self-repairing protective film. If the coating on the surface of the steel bars in the concrete is damaged, the chloride ions will cause slight corrosion of the exposed parts of the steel. At this time, the iron oxidation reaction occurs at the anode to generate iron ions, and the oxygen reduction reaction occurs at the cathode to generate hydroxide ions. Changes in the local microenvironment (ion concentration, pH value, etc.) promote the dissolution of phosphate in the releasable phosphate phase in the coating. Chloropapatite acts as a crystallization nucleus, promoting the crystallization and growth of the released phosphate and free calcium ions in the concrete pore fluid, forming a protective precipitation film on the exposed steel bar surface, hindering the further development of corrosion.
[0016] In summary, the present invention has the following advantages and outstanding technical effects: (1) It is a pure inorganic material, and there is no change in the xenon lamp aging test for 8000 hours, and the coating itself has excellent durability; (2) The hardness of the coating is high, reaching 300-1000HV, which is conducive to reducing the bonding slip between the steel bar and the concrete; (3) The coating remains stable in concrete without chloride ion pollution. When chloride ions reach the surface of the coating, the coating can fix chloride ions to reduce steel corrosion; (4) In the case of coating damage and chloride ion corrosion, a protective precipitation film will be formed in the damaged area, which has the effect of self-repair of damage. (5) It has a wide range of applications and is suitable for the corrosion protection of steel bars in concrete structures, and is also suitable for the corrosion protection of steel or other metals in other alkaline and chloride ion corrosion environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 These are pictures of Examples 1-3 of the present invention after 8000 hours of xenon lamp aging test.
[0018] Figure 2 This is the EDS spectrum of chlorapatite on the surface of Example 1 of the present invention.
[0019] Figure 3 The development and changes of the surface of Example 2 of the present invention when immersed in concrete pore fluid. DETAILED DESCRIPTION
[0020] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention are described illustratively below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0021] Example 1
[0022] An inorganic anticorrosive coating with dual functions of chloride ion fixation and damage self-repair includes the following components by weight: 50 grams of sodium borate, 25 grams of potassium borate, 50 grams of sodium carbonate, 50 grams of sodium silicate, 25 grams of calcium fluoride, 125 grams of hydroxy calcium apatite, 50 grams of sodium phosphate, 25 grams of potassium phosphate, 50 grams of zinc phosphate, 25 grams of boron oxide, and 25 grams of bismuth oxide. It is applied to the surface of steel bars at a high temperature of 680°C, and the coating thickness is 225μm.
[0023] Example 2
[0024] An inorganic anticorrosive coating with dual functions of chloride ion fixation and damage self-repair includes the following components by weight: 25 grams of sodium borate, 75 grams of potassium carbonate, 40 grams of sodium silicate, 10 grams of calcium fluoride, 100 grams of hydroxy magnesium apatite, 100 grams of hydroxy sodium apatite, 75 grams of magnesium phosphate, 25 grams of boron oxide, 25 grams of phosphorus pentoxide, and 25 grams of bismuth oxide. It is applied to the surface of steel bars at a high temperature of 550°C, and the coating thickness is 60μm.
[0025] Example 3
[0026] An inorganic anticorrosive coating with dual functions of chloride ion fixation and damage self-repair includes the following components by weight: 25 grams of potassium borate, 100 grams of sodium carbonate, 75 grams of potassium carbonate, 100 grams of sodium silicate, 25 grams of calcium fluoride, 25 grams of hydroxy calcium apatite, 25 grams of hydroxy potassium apatite, 25 grams of sodium phosphate, 25 grams of zinc phosphate, 35 grams of phosphorus pentoxide, and 40 grams of zinc oxide. After being coated on the surface of steel bars at a high temperature of 410°C, the coating thickness is 475μm.
[0027] In order to verify the implementation effect of the present invention, the following experiments were carried out.
[0028] (1) Coating hardness
[0029] The hardness of the coating was tested using a microhardness tester equipped with a Vickers indenter. The load dwell time was 10s and the indentation load was 0.98N. The microhardness was calculated as follows:
[0030]
[0031] Where HV is the Vickers hardness, in MPa; F is the indentation load, in N; S is the indentation projection area, in mm 2 ; α is the angle between the indenter faces (136° for Vickers indenter); d is the average length of the indentation diagonal, in mm.
[0032] Through calculation, the hardness of the coatings in Example 1, Example 2 and Example 3 are 975 HV, 620 HV and 330 HV respectively.
[0033] (2) Xenon lamp aging test
[0034] The xenon lamp artificial weathering test device was used to continuously aging the steel bar with the xenon lamp for 8000 hours, and the surface morphology of the coated steel bar was observed. Figure 1 It can be seen that after 8000h of xenon lamp aging, the surfaces of Examples 1-3 did not undergo any changes, indicating that the coatings of the present invention have excellent durability, which is mainly because the coating materials of the present invention are all pure inorganic aging-resistant materials.
[0035] (3) Chloride ion fixation performance
[0036] The coated steel bars of Examples 1-3 were immersed in a mixed solution of saturated calcium hydroxide and 5wt% sodium chloride at a pH of 12.7 to simulate the pore solution of concrete. After immersion for 30 days, the coating surface was analyzed by energy spectrum, and the concentration of chloride ions in the solution was tested. Chlorapatite phase was detected on the surface of Examples 1-3 by energy spectrum, and the representative results are shown in FIG. Figure 2 In addition, ion analysis shows that the chloride ion concentration of the solution of Example 1, Example 2 and Example 3 is reduced to 17%, 8% and 21% of the original, respectively. This shows that under the conditions of alkaline pore fluid and chloride ions in concrete, the hydroxyapatite phase in the coating is activated, and it reacts with chloride ions to form chlorapatite, which has the effect of fixing chloride ions and consuming corrosive chloride ions, thereby effectively reducing the corrosion of steel bars.
[0037] (4) Damage self-repair performance
[0038] The partially damaged coated steel bars of Examples 1-3 were immersed in saturated calcium hydroxide with a pH of 12.7 for 40 days, and then 5wt% sodium chloride was added to prepare a mixed solution simulating concrete pores, and the morphological changes at the coating defects were observed by optical microscopy. In a single saturated calcium hydroxide solution, the coating damage of Examples 1-3 did not undergo significant changes; after adding sodium chloride, protective damage self-repairing films appeared at the coating damage of Examples 1-3. Representative results are shown in Figure 2. Figure 3 The above results show that in the concrete pore solution with chloride ions, changes in the local microenvironment (ion concentration, pH value, etc.) will promote the dissolution of phosphate in the releasable phosphate phase in the coating. At this time, chlorapatite is used as a crystallization nucleus to promote the crystallization and growth of phosphate and calcium ions in the concrete pore solution, forming a protective precipitation film on the exposed steel bar surface, hindering the further development of corrosion.
Claims
1. An inorganic anticorrosive coating having the dual functions of chloride ion fixation and damage self-repair, comprising the following components by weight: 30 to 70 parts of a matrix phase, 10 to 40 parts of a hydroxyapatite phase, 10 to 30 parts of a phosphate phase, and 10 to 20 parts of a flux phase; a portion of the phosphate phase can interact with the matrix phase to form a basic film-forming material, forming a non-releasable phosphate phase that is not easily dissolved during the service of the coating; another portion of the phosphate phase is distributed in the basic film-forming material through a filling effect, and is dissolved under specific inducing conditions to form a releasable phosphate phase.
2. The inorganic anticorrosion coating having the dual functions of chloride ion fixation and damage self-repair according to claim 1, characterized in that: The matrix phase consists of three parts. The first part is any one of sodium borate and potassium borate or a combination of two of them. The second part is any one of sodium carbonate and potassium carbonate or a combination of two of them. The third part is sodium silicate and calcium fluoride.
3. The inorganic anticorrosion coating having the dual functions of chloride ion fixation and damage self-repair according to claim 1, characterized in that: The hydroxyapatite phase is any one or a combination of two or more of hydroxy calcium apatite, hydroxy magnesium apatite, hydroxy sodium apatite, hydroxy potassium apatite and derivatives thereof.
4. The inorganic anticorrosion coating having the dual functions of chloride ion fixation and damage self-repair according to claim 1, characterized in that: The phosphate phase is any one of sodium phosphate, potassium phosphate, zinc phosphate and magnesium phosphate or a combination of two or more thereof.
5. The inorganic anticorrosion coating having the dual functions of chloride ion fixation and damage self-repair according to claim 1, characterized in that: The flux phase is any one of boron oxide, phosphorus pentoxide, bismuth oxide and zinc oxide, or a combination of two or more thereof.
6. The inorganic anticorrosion coating having the dual functions of chloride ion fixation and damage self-repair according to claim 1, characterized in that: The coating is formed by coating on the surface of the steel bar at a high temperature of 400-700° C., has a thickness of 50-500 μm and a hardness of 300-1000 HV.
Citation Information
Patent Citations
Metal anticorrosive coating and preparation method and application thereof
CN108531908A
Active inorganic anticorrosive coating for improving bonding strength between steel bar and concrete and coating method thereof
CN110484027A
Sprayable phosphate cementitious coatings and a method and apparatus for the production thereof
US20020009622A1
Inorganic phosphate corrosion resistant coatings
US20130126050A1