Preparation method of latex paint

By replacing calcined kaolin with wollastonite powder, the high cost and environmental pollution problems of calcined kaolin in latex paint preparation are solved, the moisture-proof performance and stability of latex paint are improved, and efficient latex paint production is achieved.

CN119019879APending Publication Date: 2024-11-26ANHUI NEST NEW MATERIAL TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411052053.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the existing latex paint preparation methods, the demand for calcined kaolin is large, the processing steps are cumbersome and easy to contaminate, resulting in high production costs and is unfavorable to the environment.

Method used

Use wollastonite powder instead of calcined kaolin. Mix ethylene glycol, talc, wollastonite powder, salt gypsum powder and deionized water through a dispersing cylinder and a high-speed mixer. Add additives and then add them to the mixer until uniformly, forming latex The preparation of lacquer and wollastonite powder includes selection, coarse crushing, fine grinding and ultra-fine grinding to make powder.

Benefits of technology

Wollastonite powder improves the moisture-proof performance and stability of latex paint, reduces hygroscopicity and deformation degree, and has high production efficiency. It is suitable for large-scale production and avoids environmental pollution and high costs caused by calcined kaolin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019879A_ABST
    Figure CN119019879A_ABST
Patent Text Reader

Abstract

The invention discloses a latex paint preparation method, which relates to the technical field of paint processing, and comprises the following steps: S1, raw material preparation: adding weighed ethylene glycol, talcum powder, wollastonite powder and salt gypsum powder into a dispersion cylinder, then adding deionized water, and fully and uniformly mixing to generate a colloidal substance; s2, auxiliary agent preparation: starting a high-speed stirrer, sequentially adding the pigment, the microbicide, the coalescing agent, the thickening agent, the pigment dispersing agent, the defoaming agent and the wetting agent at a low speed, and promoting uniform stirring. S3, latex paint preparation: sequentially adding the raw materials prepared in the step S1 and the step S2 and the auxiliaries into a stirrer, and then adding deionized water until the materials are uniformly stirred. The wollastonite is combined with other raw materials, so that the damp-proof performance of the latex paint is guaranteed. Meanwhile, due to the needle-like characteristic, low expansion rate and excellent thermal shock resistance, the stability of the property of the latex paint is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating processing, and in particular to a method for preparing latex paint. Background Art

[0002] The preparation method of latex paint varies depending on the raw materials used. There are mainly polyvinyl acetate latex paint, ethylene propylene latex paint, pure acrylic latex paint, etc. According to the different application environments of the products, it can be divided into two types: interior wall latex paint and exterior wall latex paint. According to the gloss effect of the decoration, it can be divided into matte, matte, semi-gloss, silky and glossy types.

[0003] Most of the existing moisture-proof latex paints use ethylene glycol, talcum powder, calcined kaolin, salt gypsum powder and deionized water as the main raw materials, which are fully mixed to form a colloidal substance, and then diatomaceous earth, mica powder, etc. are added for grinding and dispersion, and finally the remaining deionized water and other additives are added and stirred evenly.

[0004] Kaolin is a clay mineral, the main component of which is kaolinite. It has good plasticity, dispersibility, fire resistance, adhesion and stability. It has unique performance advantages such as high activity, high whiteness, high dispersion and high hiding, plus the environmental protection characteristics of non-toxicity, no radiation and no pollution. It is widely used in many fields such as papermaking, ceramics, rubber, refractory materials and agriculture. However, calcined kaolin is made of hard kaolin generated from coal seams through repeated grinding and high-temperature calcination, and loses crystal water to form a fluffy porous flaky structure. In the assembly line operation of mass production of latex paint, the demand for calcined kaolin is large, the steps in the processing process are relatively complicated, and environmental pollution is easily generated during the calcination process, and the production cost is high. Therefore, the present application provides a method for preparing latex paint to meet the demand. Summary of the invention

[0005] In view of the above problems, the present application provides a method for preparing latex paint.

[0006] To achieve the above object, the present application provides the following technical solution: a method for preparing latex paint, the method comprising the following preparation steps:

[0007] S1: Raw material preparation: add weighed ethylene glycol, talcum powder, wollastonite powder, and salt gypsum powder into a dispersion tank, and then add deionized water to mix them thoroughly and evenly to generate a colloidal substance.

[0008] S2: Preparation of additives: start the high-speed mixer, add pigment, microbicide, film-forming aid, thickener, pigment dispersant, defoamer and wetting agent in sequence at a low speed to promote uniform mixing.

[0009] S3: preparing latex paint, adding the raw materials and additives prepared in steps S1 and S2 into a stirrer in sequence, and then adding deionized water until the mixture is stirred evenly.

[0010] Furthermore, the preparation process of wollastonite powder in step S1 includes the following steps:

[0011] A1: After the wollastonite blocks are sorted and cleaned, they are put into a jaw crusher for coarse crushing;

[0012] A2: Place the coarsely crushed wollastonite blocks into a ball mill for fine grinding.

[0013] A3: The finely ground wollastonite particles are subjected to ultrafine grinding by jet milling to form wollastonite powder.

[0014] Furthermore, in the step S1, when ethylene glycol, talcum powder, wollastonite powder, salt gypsum powder and deionized water are initially mixed, the speed of the impeller is 1000-1200 r / min. After stirring for 20-30 minutes, it is necessary to adjust the distance between the impeller and the bottom wall of the dispersion cylinder so that the vortex is in a shallow basin shape. Subsequently, the speed of the impeller is controlled to 1200-1500 r / min, and stirred again for 15-20 minutes until the raw materials are evenly stirred.

[0015] Furthermore, after the high-speed stirrer in step S2 is turned on, the controller speed is 600-800 r / min, and then the microbicide, film-forming aid, thickener, pigment dispersant, defoamer, and wetting agent are added in sequence, the speed is adjusted to 1200-1500 r / min, and the stirring time is 25-30 min until the additives are evenly stirred.

[0016] Furthermore, the pigment in step S2 is mica powder.

[0017] Furthermore, the microbicide in step S2 is a hydrogen peroxide solution.

[0018] Furthermore, the thickener in step S2 is gelatin.

[0019] In summary, the technical effects and advantages of the present invention are as follows:

[0020] The present invention uses wollastonite powder to replace calcined kaolin. Wollastonite has an interference effect on the combination of plant fibers, making them insensitive to humidity, reducing their hygroscopicity and deformation, and combined with other raw materials to ensure the moisture-proof performance of latex paint. At the same time, due to its needle-like characteristics, low expansion rate and excellent thermal shock resistance, the stability of latex paint properties is improved. At the same time, the production efficiency of wollastonite powder is relatively high, and it is suitable for the working environment of preparing a large amount of latex paint. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0022] Figure 1 It is a schematic diagram of the steps of the present invention. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Embodiment 1:

[0025] refer to Figure 1 A method for preparing a latex paint is shown, the method comprising the following preparation steps:

[0026] S1: Raw material preparation: add weighed ethylene glycol, talcum powder, wollastonite powder, and salt gypsum powder into a dispersion tank, and then add deionized water to mix them thoroughly to generate a colloidal substance;

[0027] S2: Preparation of additives: start the high-speed mixer, add pigment, microbicide, film-forming additive, thickener, pigment dispersant, defoamer and wetting agent in sequence at a low speed, and stir them evenly;

[0028] S3: preparing latex paint, adding the raw materials and additives prepared in steps S1 and S2 into a stirrer in sequence, and then adding deionized water until the mixture is stirred evenly, to obtain latex paint material 1.

[0029] The preparation process of wollastonite powder in step S1 comprises the following steps:

[0030] A1: After the wollastonite blocks are sorted and cleaned, they are put into a jaw crusher for coarse crushing;

[0031] A2: Place the roughly crushed wollastonite block into a ball mill for fine grinding;

[0032] A3: The finely ground wollastonite particles are subjected to ultrafine grinding by jet milling to form wollastonite powder.

[0033] In step S1, when ethylene glycol, talcum powder, wollastonite powder, salt gypsum powder and deionized water are initially mixed, the impeller speed is 1200 r / min. After stirring for 25 minutes, it is necessary to adjust the distance between the impeller and the bottom wall of the dispersion cylinder so that the vortex is in a shallow basin shape. Subsequently, the impeller speed is controlled to 1400 r / min, and stirred again for 20 minutes until the raw materials are evenly stirred.

[0034] After the high-speed mixer is turned on in step S2, the controller speed is 800r / min, and then the microbicide, film-forming aid, thickener, pigment dispersant, defoamer, and wetting agent are added in sequence, the speed is adjusted to 14000r / min, and the stirring time is 30min until the additives are evenly stirred.

[0035] The pigment in step S2 is mica powder.

[0036] The microbicide in step S2 is a hydrogen peroxide solution.

[0037] The thickener in step S2 is gelatin.

[0038] Example 2: The wollastonite powder in Example 1 was replaced with calcined kaolin, and the other experimental conditions remained unchanged.

[0039] S1: Raw material preparation: add weighed ethylene glycol, talcum powder, calcined kaolin, salt gypsum powder into a dispersion tank, and then add deionized water to mix them thoroughly and evenly to generate a colloidal substance.

[0040] S2: Preparation of additives: Turn on the high-speed mixer and add pigment, microbicide, film-forming additive, thickener, pigment dispersant, defoamer and wetting agent in sequence at a low speed to make them stir evenly.

[0041] S3: preparing latex paint, adding the raw materials and additives prepared in steps S1 and S2 into a stirrer in sequence, and then adding deionized water until stirred evenly to obtain latex paint material 2.

[0042] In step S1, when ethylene glycol, talcum powder, calcined kaolin, salt gypsum powder and deionized water are initially mixed, the impeller speed is 1200 r / min. After stirring for 25 minutes, it is necessary to adjust the distance between the impeller and the bottom wall of the dispersion cylinder so that the vortex is in a shallow basin shape. Subsequently, the impeller speed is controlled to 1400 r / min, and stirred again for 20 minutes until the raw materials are evenly stirred.

[0043] After the high-speed mixer is turned on in step S2, the controller speed is 800r / min, and then the microbicide, film-forming aid, thickener, pigment dispersant, defoamer, and wetting agent are added in sequence, the speed is adjusted to 14000r / min, and the stirring time is 30min until the additives are evenly stirred.

[0044] According to the above experiment, two latex paint materials with different raw materials were prepared, and the latex paint materials were applied on building materials. After the latex paint materials formed into films, the waterproof ability was tested. The specific test method was: the materials were immersed in water for 48 hours, and then their water resistance was tested. The specific experimental data are as follows:

[0045]

[0046] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing latex paint, Features: The method comprises the following preparation steps: S1: Raw material preparation: add weighed ethylene glycol, talcum powder, wollastonite powder, and salt gypsum powder into a dispersion tank, and then add deionized water to mix them thoroughly to generate a colloidal substance; S2: Preparation of additives: start the high-speed mixer, add pigment, microbicide, film-forming additive, thickener, pigment dispersant, defoamer and wetting agent in sequence at a low speed, and stir them evenly; S3: preparing latex paint, adding the raw materials and additives prepared in steps S1 and S2 into a stirrer in sequence, and then adding deionized water until the mixture is stirred evenly.

2. The method for preparing latex paint according to claim 1, Features: The preparation process of wollastonite powder in step S1 comprises the following steps: A1: After the wollastonite blocks are sorted and cleaned, they are put into a jaw crusher for coarse crushing; A2: Place the roughly crushed wollastonite block into a ball mill for fine grinding; A3: The finely ground wollastonite particles are subjected to ultrafine grinding by jet milling to form wollastonite powder.

3. The method for preparing latex paint according to claim 1, Features: In the step S1, the speed of the impeller during the preliminary mixing of ethylene glycol, talcum powder, wollastonite powder, salt gypsum powder and deionized water is 1000-1200 r / min. After stirring for 20-30 minutes, it is necessary to adjust the distance between the impeller and the bottom wall of the dispersion cylinder so that the vortex is in a shallow basin shape. Subsequently, the speed of the impeller is controlled to 1200-1500 r / min, and stirring is continued for 15-20 minutes until the raw materials are evenly stirred.

4. The method for preparing latex paint according to claim 1, Features: After the high-speed stirrer in step S2 is turned on, the controller speed is 600-800 r / min, and then the microbicide, film-forming aid, thickener, pigment dispersant, defoamer, and wetting agent are added in sequence, the speed is adjusted to 1200-1500 r / min, and the stirring time is 25-30 minutes until the additives are evenly stirred.

5. The method for preparing latex paint according to claim 1, Features: The pigment in step S2 is mica powder.

6. The method for preparing latex paint according to claim 1, Features: The microbicide in step S2 is a hydrogen peroxide solution.

7. The method for preparing latex paint according to claim 1, Features: The thickener in step S2 is gelatin.

Citation Information

Patent Citations

  • Preparation method of moisture-proof latex paint

    CN107987567A

  • Outer wall latex paint and preparation method thereof

    CN109054548A

  • Emulsion paint with good environmental protection performance and preparation method thereof

    CN111019460A