High-permeability plug hole printing ink, preparation method thereof, PCB (Printed Circuit Board) and application

By using high permeability plug-in ink in PCB board, the offset, gap and crushing problems during the burial of the magnetic core are solved, and the propagation of the magnetic field is maintained, thereby achieving the improvement of electromagnetic compatibility and mechanical strength.

CN119019887APending Publication Date: 2024-11-26SHENZHEN BAROY NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411159296.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the power supply module, core deviation, gap and crushing are prone to occur when the magnetic core is buried in the PCB, and the ink plug holes will affect the propagation and distribution of the magnetic field.

Method used

High permeability plug-in ink is used, and the composition includes 88 to 89 parts of magnetic powder, 8.5 to 9.9 parts of epoxy resin, 0.5 to 1 part of curing agent and 0.5 to 2 parts of additives. The magnetic powder contains amorphous iron-based magnetic powder and neodymium iron. Boron magnetic powder, zinc oxide magnetic powder, iron-cobalt nickel magnetic powder and copper oxide magnetic powder are prepared by vacuum stirring and dispersion, filled in the holes of the PCB plate and baked and cured in hot baking.

Benefits of technology

It effectively solves the problems of core offset, gap and crushing, while maintaining the propagation and distribution of the magnetic field, improving the electromagnetic compatibility and mechanical strength of the PCB board.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005974320000091
    Figure BDA0005005974320000091
  • Figure BDA0005005974320000101
    Figure BDA0005005974320000101
Patent Text Reader

Abstract

The invention discloses high-magnetic-conductivity plug hole printing ink, a preparation method thereof, a PCB and application, and relates to the technical field of PCBs. The high-magnetic-conductivity plug hole printing ink is prepared from, by mass, 88-89 parts of magnetic powder, 8.5-9.9 parts of epoxy resin, 0.5-1 part of curing agent and 0.5-2 parts of auxiliaries. The magnetic powder comprises at least one of amorphous iron-based magnetic powder, neodymium-iron-boron magnetic powder, zinc oxide magnetic powder, iron-cobalt-nickel magnetic powder and copper oxide magnetic powder. The high-permeability hole plugging ink provided by the invention is used for plugging holes in a PCB (Printed Circuit Board), so that magnetic embedding of the PCB is realized, the surface area of the PCB is greatly reduced, the permeability of the PCB is improved, and the problems that a magnetic core deviates when the magnetic core is embedded into the PCB, a gap exists between the magnetic core and the PCB and the magnetic core is crushed are solved. Meanwhile, as the high-permeability hole plugging ink contains the magnetic powder, hole plugging does not affect propagation and distribution of a magnetic field in a material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of printed circuit boards, and in particular to a high-permeability plugging ink, a preparation method thereof, a PCB board and applications. Background Art

[0002] The power module PCB (Printed Circuit Board, Chinese name is printed circuit board) is an important part of power products. With the development of product needs, the trend of high-density miniaturization of power modules is becoming increasingly obvious. However, among the surface mount devices of power modules, the inductor element area occupies the largest surface area of ​​PCB. Therefore, the inductor element is one of the bottlenecks for the miniaturization of power products. If the inductor (including the magnetic core) is buried inside the PCB, the surface area of ​​PCB will be greatly reduced. The saved area can be used to more reasonably arrange other components, providing a good solution for the high-density miniaturization of power modules. However, the manufacturing process of high-end printed circuit boards such as high-layer boards, arbitrary-order HDI, and package carriers with various components buried is becoming more and more complicated. Correspondingly, the plugging process of heat dissipation holes and conduction holes in circuit boards has gradually developed to ink plugging, resin plugging, copper paste plugging and micro-hole filling. Filling is carried out by printing to achieve the purpose of plugging.

[0003] However, plugging is usually used to fill the through holes on the PCB to prevent contamination such as moisture and dust, or to improve the mechanical stability of the circuit. If the environment or equipment where the ink is used has a magnetic field, or the ink will directly contact the magnetic component, plugging will affect the propagation and distribution of the magnetic field in the material. Summary of the invention

[0004] The main purpose of the present invention is to provide a high magnetic permeability plugging ink, a preparation method thereof, a PCB board and an application thereof, aiming to solve the problems of magnetic core deviation when the magnetic core is buried in a PCB, a gap between the magnetic core and the PCB, and magnetic core crushing.

[0005] In order to achieve the above-mentioned object, the high magnetic permeability plugging ink proposed in the present invention comprises the following components in parts by weight:

[0006] Magnetic powder 88-89 parts;

[0007] Epoxy resin 8.5-9.9 parts;

[0008] Curing agent 0.5-1 part;

[0009] 0.5-2 parts of additives;

[0010] The magnetic powder includes at least one of amorphous iron-based magnetic powder, neodymium iron boron magnetic powder, zinc oxide magnetic powder, iron cobalt nickel magnetic powder and copper oxide magnetic powder.

[0011] In one embodiment, the amorphous iron-based magnetic powder includes amorphous iron-based magnetic powder with a particle size of 500 mesh and amorphous iron-based magnetic powder with a particle size of 250 mesh, by mass percentage;

[0012] In one embodiment, the mass ratio of the amorphous iron-based magnetic powder with a particle size of 500 mesh and the amorphous iron-based magnetic powder with a particle size of 250 mesh is (55.8-74.29): (13.87-32.36).

[0013] In one embodiment, the epoxy resin includes at least one of bisphenol A novolac epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, dicyclopentadiene phenol epoxy resin and biphenyl phenol epoxy resin.

[0014] In one embodiment, the curing agent includes at least one of an amine curing agent, an acid anhydride curing agent, and an imidazole curing agent;

[0015] The amine curing agent includes 4,4'-diaminodiphenyl sulfone and 4,4'-diaminodiphenylmethane; and / or,

[0016] The acid anhydride curing agent includes phthalic anhydride, trimellitic anhydride and maleic anhydride; and / or,

[0017] The imidazole curing agents include PN-23, PN-31, PN-40, PN-50, PN-H, 2,4-diamino-6-(2-methylimidazole-1-ethyl)-S-triazine, and 2,4-diamino-6-(2-ethyl-4-methylimidazole-1-ethyl)-S-triazine.

[0018] In one embodiment, the auxiliary agent includes at least one of a wetting and dispersing agent, an epoxy diluent, and a silane coupling agent;

[0019] The wetting and dispersing agent includes BYK-110, BYK-111, Disponer 904, Disponer 904S, Lubrizol 2400SC or Lubrizol 20000; and / or,

[0020] The epoxy diluent includes p-tert-butylphenyl glycidyl ether 693, phenyl glycidyl ether 690 or HK-66; and / or,

[0021] The silane coupling agent includes KH550, KH560 or KH580.

[0022] The present invention also provides a method for preparing a high magnetic permeability plugging ink, comprising the following steps:

[0023] The epoxy resin, the curing agent and the auxiliary agent are mixed and ground to obtain a mixture; the mixture and the magnetic powder are stirred, dispersed and degassed under vacuum conditions to obtain the high magnetic permeability plugging ink.

[0024] In one embodiment, the fineness of the mixture is less than 15 μm; and / or,

[0025] The stirring speed is 100-200 rpm; and / or,

[0026] The dispersion rotation speed is 1300-1700 rpm.

[0027] The present invention also provides a PCB board, comprising holes filled with the high magnetic permeability plugging ink.

[0028] The present invention also proposes an application of high magnetic permeability plugging ink, which is buried in the holes of a PCB board, thermally baked and cured, and then ground and polished to obtain an ink plugging PCB board.

[0029] The high magnetic permeability plugging ink provided by the present invention comprises the following components: 88-89 parts of magnetic powder, 8.5-9.9 parts of epoxy resin, 0.5-1 parts of curing agent and 0.5-2 parts of auxiliary agent. The magnetic powder comprises at least one of amorphous iron-based magnetic powder, neodymium iron boron magnetic powder, zinc oxide magnetic powder, iron cobalt nickel magnetic powder and copper oxide magnetic powder. By inserting the high magnetic permeability plugging ink into the PCB board, the problems of magnetic core offset when the magnetic core is buried in the PCB, the gap between the magnetic core and the PCB, and the crushing of the magnetic core are solved. At the same time, since the high magnetic permeability plugging ink contains magnetic powder, plugging will not affect the propagation and distribution of the magnetic field in the material. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] If there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features limited to "first" and "second" may explicitly or implicitly include at least one of the features. In addition, if "and / or" or "and / or" appears in the full text, its meaning includes three parallel schemes. Taking "A and / or B" as an example, it includes scheme A, or scheme B, or a scheme that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in the field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0032] Among the surface mount devices of current power modules, the inductor element occupies the largest surface area of ​​the PCB, so the inductor element is one of the bottlenecks in the miniaturization of power products.

[0033] The present invention proposes a high magnetic permeability plugging ink, which includes the following components by weight: 88-89 parts of magnetic powder, 8.5-9.9 parts of epoxy resin, 0.5-1 part of curing agent and 0.5-2 parts of auxiliary agent. The magnetic powder includes at least one of amorphous iron-based magnetic powder, neodymium iron boron magnetic powder, zinc oxide magnetic powder, iron cobalt nickel magnetic powder and copper oxide magnetic powder. The high magnetic permeability plugging ink contains magnetic powder, and plugging the hole will not affect the propagation and distribution of the magnetic field in the material.

[0034] In one embodiment of the present invention, the amorphous iron-based magnetic powder includes, by mass percentage, amorphous iron-based magnetic powder with a particle size of 500 mesh and amorphous iron-based magnetic powder with a particle size of 250 mesh. After the magnetic powders of different mesh sizes are mixed, the small particles can fill the gaps between the large particles, thereby increasing the overall filling density of the magnetic powder and helping to improve the magnetic permeability of the high magnetic permeability plugging ink.

[0035] In one embodiment of the present invention, the mass ratio of the amorphous iron-based magnetic powder with a particle size of 500 mesh and the amorphous iron-based magnetic powder with a particle size of 250 mesh is (55.8-74.29): (13.87-32.36). When mixed at this ratio, the magnetic powder can form a more continuous and effective magnetic flux path, reduce magnetic resistance, and increase magnetic permeability.

[0036] In one embodiment of the present invention, the mass ratio of the 500-mesh amorphous iron-based magnetic powder to the 250-mesh amorphous iron-based magnetic powder is 74.29:13.87. When mixed at this ratio, the magnetic powder can form a more continuous and effective magnetic flux path, reduce magnetic resistance, and increase magnetic permeability.

[0037] In one embodiment of the present invention, the epoxy resin includes at least one of bisphenol A novolac epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, dicyclopentadiene phenol epoxy resin and biphenyl phenol epoxy resin. Epoxy resin has good adhesion, chemical stability and thermal stability. The addition of epoxy resin can improve the mechanical strength of the high magnetic permeability plugging ink, so that the high magnetic permeability plugging ink has sufficient hardness and wear resistance after curing.

[0038] In one embodiment of the present invention, the epoxy resin is a bisphenol A novolac epoxy resin. Bisphenol A novolac epoxy resin helps the ink flow during the plugging process and is easier to fill small and complex hole structures. The electrical insulation performance of bisphenol A novolac epoxy resin is crucial to ensure the safe operation of electronic products.

[0039] In one embodiment of the present invention, the curing agent includes at least one of an amine curing agent, an acid anhydride curing agent and an imidazole curing agent;

[0040] The amine curing agent includes 4,4'-diaminodiphenyl sulfone and 4,4'-diaminodiphenylmethane; and / or,

[0041] The acid anhydride curing agent includes phthalic anhydride, trimellitic anhydride and maleic anhydride; and / or,

[0042] The imidazole curing agent includes PN-23, PN-31, PN-40, PN-50, PN-H, 2,4-diamino-6-(2-methylimidazole-1-ethyl)-S-triazine, and 2,4-diamino-6-(2-ethyl-4-methylimidazole-1-ethyl)-S-triazine. Among them, the PN-23, PN-31, PN-40, PN-50, and PN-H are commercially available products, and their sources are, for example, Japan Ajinomoto. The curing agent can not only significantly increase the curing speed of the high magnetic permeability plugging ink, thereby speeding up the production process and improving production efficiency; but also through the cross-linking effect of the curing agent, the mechanical strength of the ink can be enhanced, making it more durable during the use of the PCB board.

[0043] In one embodiment of the present invention, the curing agent is an imidazole curing agent, which can improve the fluidity and wettability of the ink, making it easier for the ink to be evenly distributed during the plugging process.

[0044] In one embodiment of the present invention, the auxiliary agent includes at least one of a wetting and dispersing agent, a defoaming agent and a silane coupling agent;

[0045] The wetting and dispersing agent includes BYK-110, BYK-111, Disponer 904, Disponer 904S, Lubrizol 2400SC or Lubrizol 20000. The addition of the wetting and dispersing agent can enhance the dispersibility and wettability of the wetting and dispersing agent, thereby ensuring that the ink uniformly fills the pores.

[0046] The defoamer includes BYK-A550, BYK-A515, BYK-A506, Dow Corning H10, Dow Corning FS80, Foamex 1495 or Foamex 842. The addition of the defoamer can effectively reduce bubbles and avoid uneven hole filling or void formation caused by bubbles.

[0047] The silane coupling agent includes KH550, KH560 or KH580. The addition of the silane coupling agent can improve the bonding force between the high magnetic permeability plugging ink and the PCB board, ensuring that the high magnetic permeability plugging ink has good bonding performance with the PCB board during the plugging process.

[0048] In one embodiment of the present invention, the auxiliary agent includes a wetting dispersant and a silane coupling agent; the mass ratio of the wetting dispersant to the silane coupling agent is (0.01-0.1): (0.3-0.7). At this ratio, the fluidity of the high magnetic permeability plugging ink is just right. If the wetting dispersant is added in excess, the viscosity of the high magnetic permeability plugging ink will decrease, affecting the stability of the ink, making it easier to flow and difficult to control. If the silane coupling agent is added in excess, the viscosity of the high magnetic permeability plugging ink will increase, affecting the fluidity and permeability, making it difficult to evenly apply or fill the ink into the through-holes of the PCB. Excessive silane coupling agent may reduce the hardness of the plugging ink, which will affect the wear resistance and impact resistance of the ink.

[0049] The present invention also proposes a method for preparing a high magnetic permeability plugging ink, which comprises the following components in parts by mass: 88-89 parts of magnetic powder, 8.5-9.9 parts of epoxy resin, 0.5-1 part of curing agent and 0.5-2 parts of auxiliary agent. The magnetic powder includes at least one of amorphous iron-based magnetic powder, neodymium iron boron magnetic powder, zinc oxide magnetic powder, iron cobalt nickel magnetic powder and copper oxide magnetic powder. Since the preparation method adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be repeated here. The preparation method comprises the following steps:

[0050] The epoxy resin, curing agent and auxiliary agent are mixed and ground according to the components to obtain a mixture; the mixture and magnetic powder are stirred, dispersed and degassed under vacuum conditions to obtain the high magnetic permeability plugging ink.

[0051] Among them, grinding is to ensure that the curing agent is evenly dispersed in the mixture. Through grinding, the particles of the curing agent become smaller and the contact area increases, which can be better mixed with the epoxy resin and additives.

[0052] In one embodiment of the present invention, the fineness of the mixture is less than 15 μm. Small fineness can better fill the tiny holes on the PCB board, ensuring that the high magnetic permeability plugging ink can evenly cover the hole wall. Small particles have a larger specific surface area and can react with other substances faster, improving the reaction efficiency. Small particle ink can form a smoother and more uniform layer when printing, improving the printing quality of the ink.

[0053] In one embodiment of the present invention, the stirring speed is 100-200 rpm, and the stirring is performed to preliminarily mix the magnetic powder and the epoxy resin; the dispersion speed is 1300-1700 rpm, and the dispersion speed is higher than the stirring speed, so that the magnetic powder and the epoxy resin are further evenly mixed, so that the obtained high magnetic permeability plugging ink has good fluidity and plugging is smoother.

[0054] The present invention also proposes a PCB board, comprising holes, which are filled with the high magnetic permeability plugging ink. The high magnetic permeability plugging ink comprises the following components by mass: 88-89 parts of magnetic powder, 8.5-9.9 parts of epoxy resin, 0.5-1 part of curing agent and 0.5-2 parts of auxiliary agent. Among them, the magnetic powder includes at least one of amorphous iron-based magnetic powder, neodymium iron boron magnetic powder, zinc oxide magnetic powder, iron cobalt nickel magnetic powder and copper oxide magnetic powder. The holes of the PCB board are filled with the high magnetic permeability plugging ink, and the plugging of the holes will not affect the propagation and distribution of the magnetic field in the material. Since this PCB board adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be repeated here.

[0055] The present invention also proposes an application of a high magnetic permeability plugging ink, wherein the high magnetic permeability plugging ink is buried in the hole of a PCB board, heat-baked and cured, and then ground and smoothed to obtain an ink plugging PCB board. The high magnetic permeability plugging ink comprises the following components by mass: 88 to 89 parts of magnetic powder, 8.5 to 9.9 parts of epoxy resin, 0.5 to 1 part of curing agent, and 0.5 to 2 parts of auxiliary agent. The magnetic powder comprises at least one of amorphous iron-based magnetic powder, neodymium iron boron magnetic powder, zinc oxide magnetic powder, iron cobalt nickel magnetic powder, and copper oxide magnetic powder. The high magnetic permeability plugging ink can effectively guide the magnetic field, reduce electromagnetic interference, and improve the electromagnetic compatibility of the PCB board. Since the PCB board adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be repeated here.

[0056] Example 1

[0057] This embodiment provides a high magnetic permeability plugging ink, and the components of the high magnetic permeability plugging ink are as follows, calculated by weight:

[0058] 74.29g amorphous iron-based magnetic powder with a particle size of 500 mesh,

[0059] 13.87g amorphous iron-based magnetic powder with a particle size of 250 mesh,

[0060] 9.70g bisphenol A novolac epoxy resin,

[0061] 0.50 g 2,4-diamino-6-(2-ethyl-4-methylimidazole-1-ethyl)-S-triazine,

[0062] 0.05g BYK-111,

[0063] 1.09g p-tert-butylphenyl glycidyl ether 693,

[0064] 0.50g KH-560.

[0065] Wherein, the amorphous iron-based magnetic powder is the amorphous soft magnetic powder CZ-1 produced by Qinhuangdao Yahao New Material Technology Co., Ltd.

[0066] The preparation method comprises the following steps:

[0067] First, bisphenol A phenolic epoxy resin, 2,4-diamino-6-(2-ethyl-4-methylimidazole-1-ethyl)-S-triazine, BYK-111, tert-butylphenyl glycidyl ether 693 and KH-560 are ground by three rollers for 3 times according to the above mass until the fineness is less than 15μm, and then transferred to a vacuum mixer, 500 mesh amorphous iron-based magnetic powder and 250 mesh amorphous iron-based magnetic powder are added, and dispersed and stirred for 2h, with a stirring speed of 150rpm and a dispersion speed of 1500rpm. Then transfer to a vacuum stirring degassing machine for degassing until no bubbles emerge from the material, and finally package the material and perform centrifugal degassing to obtain the high magnetic permeability plugging ink. Among them, the amorphous iron-based magnetic powder with a particle size of 500 mesh is the magnetic powder that passes through a 500 mesh sieve, and the amorphous iron-based magnetic powder with a particle size of 250 mesh is the magnetic powder that passes through a 250 mesh sieve.

[0068] The high magnetic permeability plugging ink is stored below 10°C before use, thawed at room temperature for at least 12 hours, and filled with holes by printing with a horizontal printer. After plugging, it is cured by heat baking and then ground flat. The plugging process is completed.

[0069] Example 2

[0070] This embodiment provides a high magnetic permeability plugging ink, which is different from the embodiment 1 in that the components of the high magnetic permeability plugging ink are: 60.00 g of amorphous iron-based magnetic powder with a particle size of 500 mesh, and 28.16 g of amorphous iron-based magnetic powder with a particle size of 250 mesh. The rest is the same as the embodiment 1.

[0071] Example 3

[0072] This embodiment provides a high magnetic permeability plugging ink, which is different from the embodiment 1 in that the components of the high magnetic permeability plugging ink are: 55.80g of amorphous iron-based magnetic powder with a particle size of 500 mesh and 32.36g of amorphous iron-based magnetic powder with a particle size of 250 mesh. The rest are the same as the embodiment 1.

[0073] Example 4

[0074] This embodiment provides a high magnetic permeability plugging ink, which is different from the embodiment 1 in that the high magnetic permeability plugging ink comprises 88.16 g of amorphous iron-based magnetic powder with a particle size of 500 mesh. The rest is the same as the embodiment 1.

[0075] Example 5

[0076] This embodiment provides a high magnetic permeability plugging ink, which is different from the embodiment 1 in that the high magnetic permeability plugging ink comprises 88.16 g of amorphous iron-based magnetic powder with a particle size of 250 mesh. The rest is the same as the embodiment 1.

[0077] Example 6

[0078] This embodiment provides a high magnetic permeability plugging ink. Compared with the embodiment 1, the difference is that the components of the high magnetic permeability plugging ink are: 88.16g of NdFeB magnetic powder (Nd2Fe 14 B). The rest is the same as in Example 1.

[0079] Example 7

[0080] This embodiment provides a high magnetic permeability plugging ink, which is different from the embodiment 1 in that the components of the high magnetic permeability plugging ink are: 74.00 g of amorphous iron-based magnetic powder with a particle size of 500 mesh, 14.00 g of amorphous iron-based magnetic powder with a particle size of 250 mesh, and 1.25 g of p-tert-butylphenyl glycidyl ether 693. The rest are the same as the embodiment 1.

[0081] Example 8

[0082] This embodiment provides a high magnetic permeability plugging ink, which is different from the embodiment 1 in that the components of the high magnetic permeability plugging ink are: 61.00 g of amorphous iron-based magnetic powder with a particle size of 500 mesh, 28.00 g of amorphous iron-based magnetic powder with a particle size of 250 mesh, and 8.86 g of bisphenol A novolac epoxy resin. The rest is the same as the embodiment 1.

[0083] Example 9

[0084] This embodiment provides a high magnetic permeability plugging ink, which is different from the embodiment 1 in that the components of the high magnetic permeability plugging ink are: 74.29g of iron-cobalt-nickel magnetic powder with a particle size of 500 mesh and 13.87g of iron-cobalt-nickel magnetic powder with a particle size of 250 mesh. The iron-cobalt-nickel magnetic powder is CF-01 from Guangzhou Xinnod Transmission Parts Co., Ltd.

[0085] The rest are the same as in Example 1.

[0086] Example 10

[0087] This embodiment provides a high magnetic permeability plugging ink, which is different from the embodiment 1 in that the components of the high magnetic permeability plugging ink are: 60.00g of iron-cobalt-nickel magnetic powder with a particle size of 500 mesh and 28.16g of iron-cobalt-nickel magnetic powder with a particle size of 250 mesh. The iron-cobalt-nickel magnetic powder is CF-01 from Guangzhou Xinnod Transmission Parts Co., Ltd.

[0088] The rest are the same as in Example 1.

[0089] Embodiment 11

[0090] This embodiment provides a high magnetic permeability plugging ink, which is different from the embodiment 1 in that the components of the high magnetic permeability plugging ink are: 74.29g of copper oxide magnetic powder with a particle size of 500 mesh and 13.87g of copper oxide magnetic powder with a particle size of 250 mesh. The rest is the same as the embodiment 1.

[0091] Example 12

[0092] This embodiment provides a high magnetic permeability plugging ink, which is different from the embodiment 1 in that the components of the high magnetic permeability plugging ink are: 60.00 g of copper oxide magnetic powder with a particle size of 500 mesh and 28.16 g of copper oxide magnetic powder with a particle size of 250 mesh. The rest is the same as the embodiment 1.

[0093] Performance Testing

[0094] The high magnetic permeability plugging inks obtained in Examples 1 to 12 were subjected to printing tests, appearance structure monitoring, reflow soldering and thermal shock tests, and magnetic permeability tests, and the results are as follows:

[0095] Table 1 Performance test

[0096]

[0097]

[0098] Among them, the printing test: the plugging ink is plugged into the holes of the high-frequency board through a printing machine. Under the condition of ensuring that the plugging holes are full, its printing efficiency is an indicator reflecting the printing performance of the ink, that is, the printing rate.

[0099] Appearance structure monitoring: Use a magnifying glass to observe whether there are hollows or depressions on the surface; take a slice to observe whether there are bubbles or cracks in the hole.

[0100] Reflow and thermal shock test: After plugging the hole, copper is plated and the sample is subjected to 6 reflow and 6 thermal shock tests (immersed in a 288°C lead-tin furnace for 10 seconds, and repeated in sequence after cooling). Then slices are taken from the sample and the changes in the structure in the hole are observed under a microscope to judge whether there is cracking, lifting or the height of the lifting.

[0101] Printability test: Execute SJ20966-2006 test standard.

[0102] As can be seen from Table 1, Example 6 exhibits poor printability due to the large oil absorption of NdFeB magnetic powder. The high magnetic permeability plugging ink prepared in Example 1 and Example 7 has better printing performance because the amorphous iron-based magnetism, iron-cobalt-nickel magnetic powder and copper oxide magnetic powder have a small oil absorption, and the magnetic conductive resin produced has better fluidity. There are no void defects on the surface of Examples 1-12, showing a good appearance structure. After copper plating, the holes all show cracking, lifting or lifting. When it is a composite amorphous iron-based magnetic powder (Example 1-Example 3, Example 7 and Example 8), it shows a large magnetic permeability. The magnetic powders of Examples 4 and 5 are all amorphous iron-based magnetic powders of a single mesh size, and the magnetic permeability shows a different degree of decrease compared with the composite magnetic powder. In the composite magnetic powder, after the magnetic powders of different mesh sizes are mixed, the small particles can fill the gaps between the large particles, which increases the overall filling density of the magnetic powder and helps to improve the magnetic permeability of the high magnetic permeability plugging ink.

[0103] Although Examples 9 and 10 are also iron-cobalt-nickel composite magnetic powders, the amorphous iron-based composite magnetic powders lack a long-range ordered lattice structure, and thus have higher magnetic permeability than crystalline iron-cobalt-nickel magnetic powders. The amorphous iron-based composite magnetic powders have a higher magnetic permeability because the magnetic domains of the amorphous structured magnetic powders are more easily rotated during the magnetization process.

[0104] The above description is only an exemplary embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the technical concept of the present invention, or direct / indirect application in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A high magnetic permeability plugging ink, characterized in that: The high magnetic permeability plugging ink comprises the following components in parts by weight: Magnetic powder 88-89 parts; Epoxy resin 8.5-9.9 parts; 0.5-1 part of curing agent; 0.5-2 parts of additives; The magnetic powder includes at least one of amorphous iron-based magnetic powder, neodymium iron boron magnetic powder, zinc oxide magnetic powder, iron cobalt nickel magnetic powder and copper oxide magnetic powder.

2. The high magnetic permeability plugging ink according to claim 1, characterized in that: In terms of mass percentage, the amorphous iron-based magnetic powder includes amorphous iron-based magnetic powder with a particle size of 500 mesh and amorphous iron-based magnetic powder with a particle size of 250 mesh.

3. The high magnetic permeability plugging ink according to claim 2, characterized in that: The mass ratio of the amorphous iron-based magnetic powder with a particle size of 500 meshes to the amorphous iron-based magnetic powder with a particle size of 250 meshes is (55.8-74.29):(13.87-32.36).

4. The high magnetic permeability plugging ink according to claim 1, characterized in that: The epoxy resin includes at least one of bisphenol A novolac epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, dicyclopentadiene phenol epoxy resin and biphenyl phenol epoxy resin.

5. The high magnetic permeability plugging ink according to claim 1, characterized in that: The curing agent includes at least one of an amine curing agent, an acid anhydride curing agent and an imidazole curing agent; The amine curing agent includes 4,4'-diaminodiphenyl sulfone and 4,4'-diaminodiphenylmethane; and / or, The acid anhydride curing agent includes phthalic anhydride, trimellitic anhydride and maleic anhydride; and / or, The imidazole curing agents include PN-23, PN-31, PN-40, PN-50, PN-H, 2,4-diamino-6-(2-methylimidazole-1-ethyl)-S-triazine, and 2,4-diamino-6-(2-ethyl-4-methylimidazole-1-ethyl)-S-triazine.

6. The high magnetic permeability plugging ink according to claim 1, characterized in that: The auxiliary agent includes at least one of a wetting and dispersing agent, an epoxy diluent and a silane coupling agent; The wetting and dispersing agent includes BYK-110, BYK-111, Disponer-904, Disponer-904S, Lubrizol 2400SC or Lubrizol 20000; and / or, The epoxy diluent includes p-tert-butylphenyl glycidyl ether 693, phenyl glycidyl ether 690 or HK-66; and / or, The silane coupling agent includes KH-550, KH-560 or KH-580.

7. A method for preparing a high magnetic permeability plugging ink according to any one of claims 1 to 6, characterized in that: The following steps are involved: The epoxy resin, the curing agent and the auxiliary agent are mixed and ground to obtain a mixture; the mixture and the magnetic powder are stirred, dispersed and degassed under vacuum conditions to obtain the high magnetic permeability plugging ink.

8. The method for preparing the high magnetic permeability plugging ink according to claim 7, characterized in that: The fineness of the mixture is less than 15 μm; and / or, The stirring speed is 100-200 rpm; and / or, The dispersion rotation speed is 1300-1700 rpm.

9. A PCB board comprising holes, wherein the holes are filled with the high magnetic permeability plugging ink according to any one of claims 1 to 6.

10. An application of a high magnetic permeability plugging ink, characterized in that: The high magnetic permeability plugging ink as described in any one of claims 1 to 6 is buried in the holes of the PCB board, thermally baked and cured, and then ground and polished to obtain the ink plugging PCB board.