Flexible modified aerogel thermal insulation coating and preparation method thereof

Through the combination of fiber-modified aerogel and silicon sol and the use of environmentally friendly film forming additives, the problems of poor mechanical properties and environmental pollution in coating preparation are solved, and efficient heat insulation and environmental protection are achieved. Flexible modified aerogel insulation coating.

CN119019895APending Publication Date: 2024-11-26JIANGSU SOBUTE NEW MATERIALS CO LTD +1

Patent Information

Application Number
CN202310587588.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing silica aerogels have poor mechanical properties during coating preparation, and the three-dimensional porous structure is destroyed during dispersion, which is prone to agglomeration. The chemicals used are harmful to the environment and the human body, making it difficult to achieve environmental protection requirements.

Method used

The preparation method of flexible modified aerogel is prepared by aging by the fibers being modified by polydopamine and mixed with silica sol to aged. Combined with aqueous acrylic emulsion and hollow glass microspheres, a uniformly dispersed viscous paste-like coating is formed to maintain Three-dimensional porous structure, using environmentally friendly film forming additives.

Benefits of technology

It significantly improves the mechanical properties and thermal insulation properties of the aerogel, has a thermal conductivity lower than that of commercially available thermal insulation coatings, has a large thermal insulation temperature difference, and the coating has good mechanical strength, avoids cracking and shedding, and meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004243892780000091
    Figure BDA0004243892780000091
  • Figure BDA0004243892780000092
    Figure BDA0004243892780000092
  • Figure BDA0004243892780000101
    Figure BDA0004243892780000101
Patent Text Reader

Abstract

The invention discloses a flexible modified aerogel thermal insulation coating and a preparation method thereof, and belongs to the technical field of thermal insulation coatings. The flexible modified aerogel thermal insulation coating is prepared from the following raw material components: flexible modified aerogel, a water-based acrylic emulsion, a coalescing agent, ethylene glycol, hollow glass microspheres and deionized water, the flexible modified aerogel is prepared by performing surface modification on fibers through polydopamine, doping the modified fibers into silica sol and performing aging; the silica sol is synthesized by hydrolyzing one or two of dialkoxy silane and trialkoxy silane under acidic and alkaline conditions. Polymer fibers or carbon fibers are subjected to polydopamine surface modification and then doped into silica sol to prepare the flexible modified aerogel, the mechanical property of the aerogel is remarkably improved, the flexible modified aerogel can be uniformly dispersed in the coating, and the three-dimensional porous network structure of the flexible modified aerogel is kept not damaged; therefore, the flexible modified aerogel heat-preservation and heat-insulation coating has excellent heat-insulation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal insulation coatings, and in particular relates to a flexible modified aerogel thermal insulation coating and a preparation method thereof. Background Art

[0002] Thermal insulation coatings are widely used in building energy conservation, petrochemicals, new energy vehicles and other fields. Silica aerogel has become a key material for thermal insulation coatings due to its excellent characteristics such as light weight, high porosity and low thermal conductivity. At present, most domestic thermal insulation coatings directly use aerogel powder, which is then supplemented with hollow glass microspheres, perlite, diatomaceous earth powder and other insulating fillers combined with film-forming substances and additives. In the preparation process of these thermal insulation coatings, most of them do not modify and optimize the aerogel, but directly use mechanical stirring to disperse it in the coating, ignoring the problem that aerogel powder is difficult to disperse and the structure is easy to collapse. Taking the invention patent of "An aerogel flame retardant thermal insulation foam coating with hierarchical pore microstructure and its preparation method" (publication number: CN110527396B) as an example, after mixing the thickening solution and the aqueous resin, the aerogel powder is directly added to obtain a creamy coating. Although this method is simple to operate and can successfully prepare a coating in good condition, it fails to take into account the poor mechanical properties of traditional aerogels, which are extremely difficult to disperse evenly in a resin mixture with high viscosity, and the three-dimensional porous structure of the aerogel is destroyed during the stirring and dispersion process, and it is easy to agglomerate. Secondly, reinforcing fibers are used in the preparation of the coating to improve the mechanical properties of the coating, but the reinforcing fibers will produce thermal conductivity in the coating, greatly reducing the thermal insulation performance of the coating. Take the invention patent of "A SiO2-Al2O3 composite aerogel self-cleaning thermal insulation coating and its application" (publication number: CN114592354A) as an example. It first prepares the SiO2-Al2O3 composite aerogel with a three-dimensional network structure by interlacing the flaky Al2O3 and the chain SiO2 skeleton. While improving the hydrophobicity of the composite aerogel, it also improves the flexibility of the aerogel. Although the dispersibility of the aerogel powder is improved to a certain extent, the method performs pH adjustment multiple times when preparing the SiO2-Al2O3 composite aerogel, and the process is relatively complicated and cumbersome. In addition, when preparing the coating, chemicals such as dichloromethane and tetrahydrofuran that are harmful to the body and the environment are used, which makes it difficult to meet the environmental protection requirements of the coating. The coating prepared by the invention is applied to the flexible fabric by dipping and rolling, and it is difficult to apply it evenly on the fabric surface. In addition, the coating uses polydimethylsiloxane as a film-forming material, and the bonding force with the flexible fabric is greatly reduced, which greatly limits its application field. In the patent "A method for preparing fiber-reinforced flexible silica aerogel", the silica aerogel is fiber-reinforced. The patent immerses the comb-shaped fibers in silica sol, and then obtains the fiber-reinforced flexible silica aerogel through further aging and solvent replacement. However, in this method, the fibers and aerogel are only physically adsorbed, and the bonding strength is poor. The structure is easily destroyed in the subsequent coating preparation process. Summary of the invention

[0003] In order to solve the problems that the existing silica aerogel has poor mechanical properties, the three-dimensional porous structure is destroyed during the dispersion process, and agglomeration is easy to occur, the present invention provides a flexible modified aerogel thermal insulation coating and a preparation method.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0005] A flexible modified aerogel thermal insulation coating, the raw materials for its preparation include the following components by weight:

[0006] Flexible modified aerogel………………………………5-20 parts,

[0007] Water-based acrylic emulsion…………………………15-30 parts,

[0008] Film-forming aid………………………………1-2 parts,

[0009] Ethylene glycol 0.5-1.5 parts,

[0010] Hollow glass microspheres………………………………10-30 parts,

[0011] Deionized water……………………………………25-40 parts,

[0012] The flexible modified aerogel is prepared by modifying the surface of fibers with polydopamine and then adding the fibers into silica sol for aging.

[0013] The silica sol is synthesized by hydrolysis of one or two of dialkoxysilane and trialkoxysilane under acidic or alkaline conditions. The specific preparation method of the silica sol can be that one or two of dialkoxysilane and trialkoxysilane are firstly hydrolyzed in an acidic water-alcohol mixed solution containing hexadecyltrimethylammonium bromide, and then polymerized in an N,N-dimethylformamide solution with a pH of 8-9.

[0014] The mass ratio of fiber, polydopamine and silica sol in the flexible modified aerogel is 0.5-2.0:5-10:10-25.

[0015] The flexible modified aerogel thermal insulation coating, its preparation raw materials also include the following components by weight:

[0016] pH adjuster………………………………0.1-0.5 parts,

[0017] Thickener………………………………0.1-0.4 parts,

[0018] Wetting agent………………………………0.2-0.5 parts,

[0019] Dispersant………………………………0.2-0.8 parts,

[0020] Defoaming agent………………………………0.3-0.7 parts,

[0021] Furthermore, the film-forming aid is one of propylene glycol, glycol ester-12, ethylene glycol butyl ether, and ethylene glycol monoacetate, or a mixture of several of them.

[0022] Furthermore, the fiber is a polymer fiber or a carbon fiber; the polymer fiber is a mixture of one or more of aramid fiber, polyester fiber, acrylic fiber, nylon fiber, spandex fiber, polypropylene fiber, vinylon fiber, chlorofiber fiber, and fluorofiber fiber.

[0023] Furthermore, the pH regulator is ammonia water or AMP-95.

[0024] Furthermore, the thickener is one of an inorganic thickener, a cellulose thickener, a nonionic hydrophobically modified polyurethane rheological thickener, and an associative polyurethane thickener; and the molecular weight of the cellulose thickener is 30,000-100,000.

[0025] Furthermore, the wetting agent is an isomeric alcohol series wetting agent.

[0026] Furthermore, the dispersant is a polycarboxylate ammonium salt type anionic dispersant.

[0027] Furthermore, the defoaming agent is a metal soap defoaming agent.

[0028] On the other hand, the present invention also provides a method for preparing the flexible modified aerogel, which specifically comprises the following steps:

[0029] (1) immersing the fiber in a Tris-HCl solution of dopamine hydrochloride for 24-36 hours to obtain a modified fiber;

[0030] (2) adding the modified fiber to the silica sol, stirring to make the fiber dispersed evenly, allowing the silica sol to form a gel at a temperature of 35-45°C, and then fully aging it, and then post-treating it to obtain a flexible modified aerogel.

[0031] The pH of the Tris-HCl solution of dopamine hydrochloride in step (1) is 8.0-8.5, and the solubility of dopamine hydrochloride is 0.2-0.5 mol / L.

[0032] On the other hand, the present invention also provides a method for preparing the flexible modified aerogel thermal insulation coating, comprising the following steps:

[0033] (1) adding a pH regulator, a thickener, a wetting agent, a dispersant and a defoaming agent to water in sequence, and after the raw materials are completely dissolved, adding an aqueous acrylic emulsion, ethylene glycol and a film-forming aid in sequence, and mixing them uniformly to obtain a mixed emulsion;

[0034] (2) Add the flexible aerogel to the mixed emulsion while stirring, continue stirring for 30-60 minutes, then add the hollow glass microspheres and continue to disperse at a low speed for 30-45 minutes. After it becomes a viscous paste, take it out to obtain the flexible modified aerogel thermal insulation coating.

[0035] The advantages and beneficial effects of the present invention compared with the prior art are:

[0036] (1) The present invention prepares a flexible modified aerogel by surface-modifying polymer fiber or carbon fiber with polydopamine and then adding the modified aerogel into silica sol, which significantly improves the mechanical properties of the aerogel. The flexible modified aerogel can be evenly dispersed in the coating and its three-dimensional porous network structure is not destroyed, so that the flexible modified aerogel thermal insulation coating has excellent thermal insulation properties.

[0037] (2) The silica sol of the present invention is polymerized from dialkoxysilane or trialkoxysilane. After hydrolysis, such silane produces a small amount of Si-OH, which reduces the bonding sites between the silica sol and the fiber. The small amount of chemical bonds and the fiber's own properties give the silica aerogel better flexibility, thereby further enhancing the mechanical properties of the aerogel. Therefore, the thermal conductivity of the prepared flexible modified aerogel thermal insulation coating is lower than that of ordinary commercially available thermal insulation coatings, and its thermal conductivity can be as low as 0.040 W / (m·k), and the thermal insulation temperature difference can reach 38°C.

[0038] (3) The thermal insulation coating prepared using the flexible modified aerogel in the present invention has good mechanical strength. The rich fiber network in the aerogel helps to enhance the mechanical properties of the thermal insulation coating. Compared with ordinary commercially available thermal insulation coatings, there is no cracking, falling off and the like. DETAILED DESCRIPTION

[0039] In order to make the technical solutions, advantages and objectives of the present invention clearer, the present invention is described in detail through specific embodiments below. The embodiments are merely illustrative and do not limit the scope of patent protection of the present invention. Any non-essentially equivalent changes or adjustments made according to the above-mentioned invention content and spirit are within the scope of protection of the present invention.

[0040] In the embodiments and comparative examples, AMP-95 is produced by Dow Chemical; hydroxyethyl cellulose ether has a molecular weight of 30,000 and is produced by Ashland; bentonite BENTONE is produced by Hemmings and PUR-62 thickener is produced by Mingling; RW-8 thickener is produced by Dow Chemical; 3307 wetting agent is produced by Sasol; BYK349 ​​wetting agent is produced by BYK; TEGO-500 wetting agent 9 is produced by Digo; SN5027 dispersant is produced by Nopco; BYK190 dispersant is produced by BYK and 760W dispersant is produced by Ashland; NXZ defoamer is produced by Nopco; 2410AG defoamer is produced by BASF and BYK028 defoamer is produced by BYK; 7026G water-based acrylic emulsion is produced by BASF; IC-1002 water-based acrylic emulsion is produced by Dow Chemical and 7039 water-based acrylic emulsion is produced by BASF.

[0041] Example 1

[0042] The present invention discloses a flexible modified aerogel thermal insulation coating and a preparation method thereof, comprising the following steps:

[0043] Step 1, weighing 0.5 g of aramid fiber and ultrasonically cleaning it in deionized water and methanol respectively, taking it out and drying it for 12 hours, and then soaking it in a solution of 0.01 g of dopamine hydrochloride dissolved in 5 mL of Tris-HCl with a pH of 8.5 for 24 hours;

[0044] Step 2, dissolve 0.4 g of hexadecyltrimethylammonium bromide in a mixed solution of 8 mL of methanol and 12 mL of glacial acetic acid, stir at 30°C until completely dissolved, then add 3 mL of methyltrimethoxysilane, 2 mL of dimethyldimethoxysilane and 10 mL of N,N-dimethylformamide in sequence, continue stirring for 1 hour, and adjust the pH value of the mixed solution to 8 with aqueous ammonia.

[0045] Step 3, adding the treated fibers in step 1 to the mixed solution in step 2, stirring thoroughly to make the fibers evenly dispersed, and then placing in a 35°C constant temperature water bath until gel is formed, and then aging for 6 hours;

[0046] Step 4, the aged gel in step 3 is subjected to solvent replacement using isopropanol and n-hexane respectively, and finally dried at 30° C. for 12 h and 40° C. for 24 h under normal pressure, and after drying, a flexible modified aerogel is prepared.

[0047] Step 5, add 0.1 parts of AMP-95, 0.1 parts of hydroxyethyl cellulose ether, 0.2 parts of 3307 wetting agent, 0.2 parts of SN5027 dispersant and 0.3 parts of NXZ defoamer in 25 parts of deionized water in turn, stir well to make them completely dissolved, then add 30 parts of 7026G water-based acrylic emulsion, 0.5 parts of ethylene glycol and 1 part of alcohol lipid-12 film-forming aid in turn, stir well again to mix them evenly.

[0048] Step 6, add 5 parts of flexible modified aerogel to the mixed emulsion of step 5 while stirring at a speed of 350r / min, continue stirring for 30 minutes, then add 10 parts of hollow glass microspheres and continue to disperse at a low speed for 30 minutes to form a viscous paste coating, and finally take it out to complete the preparation of the thermal insulation coating.

[0049] Example 2

[0050] The present invention discloses a flexible modified aerogel thermal insulation coating and a preparation method thereof, comprising the following steps:

[0051] Step 1, weighing 1.0 g of aramid fiber and ultrasonically cleaning it in deionized water and methanol respectively, taking it out and drying it for 12 hours, and then soaking it in 0.02 g of dopamine hydrochloride dissolved in 10 mL of Tris-HCl solution with a pH of 8.5 for 30 hours;

[0052] Step 2, dissolve 0.4 g of hexadecyltrimethylammonium bromide in a mixed solution of 8 mL of methanol and 12 mL of glacial acetic acid, stir at 30°C until completely dissolved, then add 3 mL of methyltrimethoxysilane, 2 mL of dimethyldimethoxysilane and 10 mL of N,N-dimethylformamide in sequence, continue stirring for 1 hour, and adjust the pH value of the mixed solution to 9 with aqueous ammonia.

[0053] Step 3, adding the treated fibers in step 1 to the mixed solution in step 2, stirring thoroughly to make the fibers evenly dispersed, and then placing in a 40° C. constant temperature water bath until gel is formed, and then aging for 6 hours;

[0054] Step 4, the aged gel in step 3 is subjected to solvent replacement using isopropanol and n-hexane respectively, and finally dried at 30° C. for 12 h and 40° C. for 24 h under normal pressure. After drying, a flexible modified aerogel is prepared.

[0055] Step 5, add 0.25 parts of ammonia water, 0.2 parts of bentonite BENTONE, 0.25 parts of BYK349 ​​wetting agent, 0.4 parts of BYK190 dispersant and 0.5 parts of 2410AG defoamer to 35 parts of deionized water in sequence, stir well to make them completely dissolved, then add 20 parts of 7039 water-based acrylic emulsion, 1 part of ethylene glycol and 1.5 parts of propylene glycol film-forming aids in sequence, stir well again to make them evenly mixed.

[0056] Step 6, add 15 parts of flexible aerogel to the mixed emulsion of step 5 while stirring at a speed of 350r / min, continue stirring for 30 minutes, then add 20 parts of hollow glass microspheres and continue to disperse at a low speed for 35 minutes. After it becomes a viscous paste, take it out to complete the preparation of the thermal insulation coating.

[0057] Example 3

[0058] The present invention discloses a flexible modified aerogel thermal insulation coating and a preparation method thereof, comprising the following steps:

[0059] Step 1, weighing 2.0 g of aramid fiber, ultrasonically cleaning it in deionized water and methanol respectively, taking it out and drying it for 12 hours, and then soaking it in a solution of 0.05 g of dopamine hydrochloride dissolved in 15 mL of Tris-HCl with a pH of 8.5 for 36 hours;

[0060] Step 2, dissolve 0.4 g of hexadecyltrimethylammonium bromide in a mixed solution of 8 mL of methanol and 12 mL of glacial acetic acid, stir at 30°C until completely dissolved, then add 3 mL of methyltrimethoxysilane, 2 mL of dimethyldimethoxysilane and 10 mL of N,N-dimethylformamide in sequence, continue stirring for 1 hour, and adjust the pH value of the mixed solution to 8.5 with aqueous ammonia.

[0061] Step 3, adding the treated fibers in step 1 to the mixed solution in step 2, stirring thoroughly to make the fibers evenly dispersed, and then placing in a 40° C. constant temperature water bath until gel is formed, and then aging for 6 hours;

[0062] Step 4, the aged gel in step 3 is subjected to solvent replacement using isopropanol and n-hexane respectively, and finally dried at 30° C. for 12 h and 40° C. for 24 h under normal pressure. After drying, a flexible modified aerogel is prepared.

[0063] Step 5, add 0.5 parts of AMP-95, 0.4 parts of PUR-62 thickener, 0.5 parts of TEGO-500 wetting agent, 0.8 parts of 760W dispersant and 0.7 parts of BYK028 defoamer in 40 parts of deionized water in turn, stir well to make them completely dissolved, then add 30 parts of IC-1002 water-based acrylic emulsion, 1.5 parts of ethylene glycol and 2 parts of ethylene glycol ethyl ether film-forming aid in turn, stir well again to make them evenly mixed.

[0064] Step 6, add 20 parts of flexible aerogel to the mixed emulsion of step 5 while stirring at a speed of 350r / min, continue stirring for 60min, then add 30 parts of hollow glass microspheres and continue to disperse at a low speed for 45min. After it becomes a viscous paste, take it out to complete the preparation of the thermal insulation coating.

[0065] Example 4

[0066] The present invention discloses a flexible modified aerogel thermal insulation coating and a preparation method thereof, comprising the following steps:

[0067] Step 1, weighing 1.0 g of nylon fiber and ultrasonically cleaning it in deionized water and methanol respectively, taking it out and drying it for 12 hours, and then soaking it in a solution of 0.01 g of dopamine hydrochloride dissolved in 5 mL of Tris-HCl with a pH of 8.5 for 24 hours;

[0068] Step 2, dissolve 0.4 g of hexadecyltrimethylammonium bromide in a mixed solution of 8 mL of methanol and 12 mL of glacial acetic acid, stir at 30°C until completely dissolved, then add 3 mL of methyltrimethoxysilane, 2 mL of dimethyldimethoxysilane and 10 mL of N,N-dimethylformamide in sequence, continue stirring for 1 hour, and adjust the pH value of the mixed solution to 8 with aqueous ammonia.

[0069] Step 3, adding the treated fibers in step 1 to the mixed solution in step 2, stirring thoroughly to make the fibers evenly dispersed, and then placing in a 40° C. constant temperature water bath until gel is formed, and then aging for 6 hours;

[0070] Step 4, the aged gel in step 3 is subjected to solvent replacement using isopropanol and n-hexane respectively, and finally dried at 30° C. for 12 h and 40° C. for 24 h under normal pressure. After drying, a flexible modified aerogel is prepared.

[0071] Step 5, add 0.5 parts of ammonia water, 0.4 parts of RW-8 thickener, 0.5 parts of 3307 wetting agent, 0.8 parts of SN5027 dispersant and 0.7 parts of NXZ defoamer to 40 parts of deionized water in sequence, stir well to make them completely dissolved, then add 30 parts of 7026G water-based acrylic emulsion, 1.5 parts of ethylene glycol and 2 parts of alcohol lipid-12 film-forming aid in sequence, stir well again to make them evenly mixed.

[0072] Step 6, add 20 parts of flexible aerogel to the mixed emulsion of step 5 while stirring at a speed of 350r / min, continue stirring for 60min, then add 30 parts of hollow glass microspheres and continue to disperse at a low speed for 45min. After it becomes a viscous paste, take it out to complete the preparation of the thermal insulation coating.

[0073] Example 5

[0074] The present invention discloses a flexible modified aerogel thermal insulation coating and a preparation method thereof, comprising the following steps:

[0075] Step 1, weighing 1.0 g of acrylic fiber and ultrasonically cleaning it in deionized water and methanol respectively, taking it out and drying it for 12 hours, and then soaking it in a solution of 0.01 g of dopamine hydrochloride dissolved in 5 mL of Tris-HCl with a pH of 8.5 for 24 hours;

[0076] Step 2, dissolve 0.4 g of hexadecyltrimethylammonium bromide in a mixed solution of 8 mL of methanol and 12 mL of glacial acetic acid, stir at 30°C until completely dissolved, then add 3 mL of methyltrimethoxysilane, 2 mL of dimethyldimethoxysilane and 10 mL of N,N-dimethylformamide in sequence, continue stirring for 1 hour, and adjust the pH value of the mixed solution to 8 with aqueous ammonia.

[0077] Step 3, adding the treated fibers in step 1 to the mixed solution in step 2, stirring thoroughly to make the fibers evenly dispersed, and then placing in a 40° C. constant temperature water bath until gel is formed, and then aging for 6 hours;

[0078] Step 4, the aged gel in step 3 is subjected to solvent replacement using isopropanol and n-hexane respectively, and finally dried at 30° C. for 12 h and 40° C. for 24 h under normal pressure. After drying, a flexible modified aerogel is prepared.

[0079] Step 5, 0.1 parts of AMP-95, 0.1 parts of hydroxyethyl cellulose ether, 0.2 parts of BYK349 ​​wetting agent, 0.2 parts of BYK190 dispersant and 0.3 parts of NXZ defoamer are added to 25 parts of deionized water in sequence, and stirred thoroughly to completely dissolve them. Then, 15 parts of 7026G water-based acrylic emulsion, 0.5 parts of ethylene glycol and 1 part of ethylene glycol film-forming aid are added in sequence, and stirred thoroughly again to mix them evenly.

[0080] Step 6, add 5 parts of flexible aerogel to the mixed emulsion of step 5 while stirring at a speed of 350r / min, continue stirring for 30 minutes, then add 10 parts of hollow glass microspheres and continue to disperse at a low speed for 30 minutes. After it becomes a viscous paste, take it out to complete the preparation of the thermal insulation coating.

[0081] Comparative Example 1

[0082] This comparative example is set based on Example 1, and the difference from Example 1 is that the thermal insulation coating prepared without adding aerogel. Compared with Example 1, only steps 5 and 6 are performed, and the addition of flexible aerogel in step 6 is cancelled. Other conditions for preparing the thermal insulation coating are the same as those in Example 1.

[0083] Comparative Example 2

[0084] This comparative example is set based on Example 1, and the difference from Example 1 is that only steps 2-6 are performed, and the addition of fibers in step 3 is cancelled. Other conditions are consistent with those for preparing the thermal insulation coating in Example 1.

[0085] Comparative Example 3

[0086] This comparative example is set based on Example 1, and the difference between it and Example 1 is that the process of modifying the aramid fiber with polydopamine in step 1 is cancelled, and the aramid fiber is directly added to the silica sol. The other steps are the same as those in Example 1.

[0087] Comparative Example 4

[0088] This comparative example is set up based on Example 1. The difference between this comparative example and Example 1 is that the homemade silica sol in step (2) of Example 1 is directly replaced by commercially available silica sol, and the other steps are the same as those of Example 1.

[0089] Comparative Example 5

[0090] Commercially available hydrophobic aerogels.

[0091] Comparative Example 6

[0092] Commercially available thermal insulation coatings.

[0093] Application Example 1

[0094] The compressive strength test was performed on the flexible aerogels prepared in Examples 1 to 5 and Comparative Examples 2 to 5 and the commercially available hydrophobic aerogels. The test results are shown in Table 1 below:

[0095] Table 1 Comparison of aerogel compressive strength test results

[0096]

[0097] As can be seen from Table 1, the compressive strength of the fiber-reinforced aerogel is significantly greater than that of the commercially available hydrophobic aerogel, indicating that fiber reinforcement helps to improve the flexibility of the aerogel. In addition, the compressive strength of the aerogel without polydopamine-modified fiber modification is also significantly lower than that of the aerogel with polydopamine-modified fiber modification.

[0098] Application Example 2

[0099] The thermal insulation coatings prepared in Examples 1 to 5, Comparative Examples 1 to 4 and Comparative Example 6 were tested for thermal conductivity with reference to GB / T25261-2018 "Reflective Thermal Insulation Coatings for Buildings". The specific testing process is as follows: The prepared thermal insulation coating is molded into a 30*30*1.5 cm test specimen in a special mold, and the thermal conductivity of the specimen is tested using the steady-state method after it is dried. The prepared thermal insulation coating is scraped and applied to a 20*30 cm asbestos-free fiber cement board, and the apparent state of the coating is observed by visual inspection. The thermal conductivity test results and the apparent state of the coating are shown in Table 2 below:

[0100] Table 2 Comparison of thermal conductivity test results and coating appearance

[0101]

[0102] As can be seen from Table 2, the thermal conductivity of the fiber-reinforced aerogel thermal insulation coating is significantly lower than that of the non-aerogel and commercially available aerogel thermal insulation coatings. In addition, the thermal insulation coating prepared by the fiber-modified aerogel did not show cracking, while the coating prepared by the non-fiber-modified aerogel and the commercially available thermal insulation coating showed different degrees of cracking, indicating that the fiber-flexible modified aerogel can significantly improve the mechanical strength of the coating.

[0103] Application Example 3

[0104] The thermal insulation coatings prepared in Examples 1 to 5, Comparative Examples 1 to 4 and Comparative Example 6 were subjected to thermal insulation temperature difference test with reference to GB / T25261-2018 "Reflective Thermal Insulation Coatings for Buildings". The specific test process is as follows: The prepared thermal insulation coating was scraped onto a 7.0*7.0*0.5 cm asbestos-free fiber cement board, and the thermal insulation temperature difference test was performed after it was dried. The thermal insulation temperature difference test results are shown in the following table:

[0105] Table 3 Comparison of thermal conductivity test results

[0106]

[0107] It can be seen from Table 3 that the thermal insulation temperature difference of the fiber reinforced aerogel thermal insulation coating is significantly greater than the thermal insulation temperature difference of the aerogel-free and commercially available aerogel thermal insulation coatings.

Claims

1. A flexible modified aerogel thermal insulation coating, It is characterized in that The raw materials for its preparation include the following components by weight: Flexible modified aerogel………………………………5-20 parts, Water-based acrylic emulsion…………………………15-30 parts, Film-forming aid………………………………1-2 parts, Ethylene glycol 0.5-1.5 parts, Hollow glass microspheres………………………………10-30 parts, Deionized water……………………………………25-40 parts, The flexible modified aerogel is prepared by modifying the surface of fibers with polydopamine and then mixing the fibers into silica sol for aging; the silica sol is synthesized by hydrolysis of one or two of dialkoxysilane and trialkoxysilane under acidic or alkaline conditions.

2. According to the flexible modified aerogel thermal insulation coating of claim 1, It is characterized in that The mass ratio of fiber, polydopamine and silica sol in the flexible modified aerogel is 0.5-2.0:5-10:10-25.

3. According to the flexible modified aerogel thermal insulation coating of claim 1, It is characterized in that The raw materials for its preparation also include the following components by weight: pH adjuster………………………………0.1-0.5 parts, Thickener………………………………0.1-0.4 parts, Wetting agent………………………………0.2-0.5 parts, Dispersant………………………………0.2-0.8 parts, Defoaming agent………………………………0.3-0.7 part.

4. According to the flexible modified aerogel thermal insulation coating of claim 1, It is characterized in that The film-forming aid is one of propylene glycol, alcohol ester-12, ethylene glycol butyl ether, and ethylene glycol monoacetate, or a mixture of the two or more thereof.

5. According to the flexible modified aerogel thermal insulation coating of claim 1, It is characterized in that The fiber is a polymer fiber or a carbon fiber; the polymer fiber is a mixture of one or more of aramid fiber, polyester fiber, acrylic fiber, nylon fiber, spandex fiber, polypropylene fiber, vinylon fiber, chloroprene fiber and fluorocarbon fiber.

6. According to the flexible modified aerogel thermal insulation coating of claim 3, It is characterized in that The pH regulator is ammonia water or AMP-95.

7. According to claim 3, the flexible modified aerogel thermal insulation coating, It is characterized in that The thickener is one of an inorganic thickener, a cellulose thickener, a nonionic hydrophobically modified polyurethane rheological thickener, and an associative polyurethane thickener; the molecular weight of the cellulose thickener is 30,000-100,000.

8. According to the flexible modified aerogel thermal insulation coating of claim 3, It is characterized in that The wetting agent is an isomeric alcohol series wetting agent, the dispersant is a polycarboxylate ammonium salt type anionic dispersant, and the defoaming agent is a metal soap defoaming agent.

9. The flexible modified aerogel thermal insulation coating according to claim 1, It is characterized in that The method for preparing the flexible modified aerogel specifically comprises the following steps: (1) immersing the fiber in a Tris-HCl solution of dopamine hydrochloride for 24-36 hours to obtain a modified fiber; (2) adding the modified fiber to the silica sol, stirring to make the fiber dispersed evenly, allowing the silica sol to form a gel at a temperature of 35-45°C, and then fully aging it, and then post-treating it to obtain a flexible modified aerogel.

10. The flexible modified aerogel thermal insulation coating according to claim 9, It is characterized in that The pH of the Tris-HCl solution of dopamine hydrochloride in step (1) is 8.0-8.5, and the solubility of dopamine hydrochloride is 0.2-0.5 mol / L.

11. A method for preparing the flexible modified aerogel thermal insulation coating according to any one of claims 1 to 10, It is characterized in that The steps include: (1) adding a pH regulator, a thickener, a wetting agent, a dispersant and a defoaming agent to water in sequence, and after the raw materials are completely dissolved, adding an aqueous acrylic emulsion, ethylene glycol and a film-forming aid in sequence, and mixing them uniformly to obtain a mixed emulsion; (2) Add the flexible aerogel to the mixed emulsion while stirring, continue stirring for 30-60 minutes, then add the hollow glass microspheres and continue to disperse at a low speed for 30-45 minutes. After it becomes a viscous paste, take it out to obtain the flexible modified aerogel thermal insulation coating.

Citation Information

Patent Citations

  • Piezoresistive sensor material and preparation method and application thereof

    CN110776667A

  • Metal surface composite SiO2 aerogel coating and preparation method thereof

    CN114806300A

  • Piezoresistive sensor material and preparation method and use thereof

    US20210143321A1

  • Aerogel Based on Gas Vesicles and Bacterial Cellulose

    US20220401908A1

Cited By

  • Inorganic water-based aerogel thermal insulation coating and preparation method thereof