Toughened glass based on antibacterial coating and preparation method thereof

By spraying antibacterial coatings formed by chemical bonds of antibacterial agents and fillers on tempered glass, the problem of insufficient antibacterial treatment in places with high hygiene requirements is solved, and the excellent antibacterial and weather resistance of tempered glass is achieved, which enhances the market Competitiveness.

CN119019900AInactive Publication Date: 2024-11-26DONGGUAN TAIRUN GLASS TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411181841.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing tempered glass lacks effective antibacterial treatment in places with high sanitary requirements, making it difficult to meet consumers' health and environmental protection needs.

Method used

Using a tempered glass preparation method based on antibacterial coating, the coating consists of polyacrylic resin, antibacterial agent, filler, etc. The antibacterial agent is prepared through specific synthesis steps to form a quaternary ammonium salt antibacterial agent. , and form chemical bonds with fillers to improve the adhesion and stability of the coating.

Benefits of technology

It achieves excellent adhesion and antibacterial properties between antibacterial coatings and tempered glass, ensures the long-term stable antibacterial properties and weather resistance of tempered glass, and enhances hygiene conditions and market competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012403040000031
    Figure BDA0005012403040000031
  • Figure BDA0005012403040000032
    Figure BDA0005012403040000032
  • Figure BDA0005012403040000041
    Figure BDA0005012403040000041
Patent Text Reader

Abstract

The invention discloses tempered glass based on an antibacterial coating and a preparation method of the tempered glass, and belongs to the technical field of glass. The preparation method comprises the following steps: stirring 40 to 50 parts of polyacrylic resin, 35 to 55 parts of a solvent, 30 to 40 parts of polyurethane resin, 15 to 20 parts of a filler, 1 to 3 parts of a coalescing agent, 0.8 to 1.2 parts of an antibacterial agent, 0.5 to 1 part of a dispersing agent, 0.4 to 0.8 part of a thickening agent, 0.2 to 0.4 part of a defoaming agent and 0.05 to 0.1 part of a flatting agent to obtain an antibacterial coating; and putting the plate glass into a toughening furnace, heating to 650-750 DEG C, cooling to 200 DEG C, taking out, spraying the antibacterial coating onto the surface of the glass, and cooling to room temperature, thereby obtaining the toughened glass. According to the present invention, the adhesion between the antibacterial coating and the tempered glass is excellent, the compatibility between the antibacterial agent and other raw materials is good, and the antibacterial agent and the filler are chemically bonded, such that the antibacterial agent and the filler can completely provide effects, and the tempered glass has excellent and stable antibacterial property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of glass, and in particular, relates to tempered glass based on an antibacterial coating and a preparation method thereof. Background Art

[0002] Tempered glass is a type of safety glass and a prestressed glass. In order to increase the strength of the glass, chemical or physical methods are usually used to form compressive stress on the glass surface. When the glass is subjected to external force, the surface stress is first offset, thereby increasing the bearing capacity and enhancing the glass's own resistance to wind pressure, cold and heat, impact, etc.

[0003] Tempered glass has many advantages. First, safety. When the glass is damaged by external force, the fragments will become small obtuse-angled particles similar to honeycombs, which are not easy to cause serious harm to the human body. Second, high strength. The impact strength of tempered glass of the same thickness is 3 to 5 times that of ordinary glass, and the bending strength is 3 to 5 times that of ordinary glass. Third, thermal stability. Tempered glass has good thermal stability and can withstand a temperature difference of 3 times that of ordinary glass, and can withstand a temperature difference of 300°C.

[0004] Antibacterial treatment of tempered glass is particularly important in daily use, especially in places with high hygiene requirements, such as hospitals and laboratories. Antibacterial treatment of tempered glass can effectively improve the hygiene of the use environment and ensure people's health and safety. Glass products that have undergone antibacterial treatment have higher market competitiveness, can meet consumers' needs for health and environmental protection, and are widely used in home, office, medical, catering and other fields to improve people's quality of life. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a tempered glass based on an antibacterial coating and a preparation method thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing tempered glass based on an antibacterial coating comprises the following steps: placing the flat glass after cutting, edge grinding, washing and drying into a tempering furnace and heating it to 650-750°C, then placing the flat glass into a quenching chamber for cooling, taking it out when the temperature drops to 200°C, spraying the antibacterial coating evenly onto the surface of the glass, and cooling it to room temperature to prepare the tempered glass based on the antibacterial coating.

[0008] Furthermore, the antibacterial coating is prepared by the following steps:

[0009] 40-50 parts of polyacrylic acid resin, 35-55 parts of solvent, 30-40 parts of polyurethane resin, 15-20 parts of filler, 1-3 parts of film-forming aid, 0.8-1.2 parts of antibacterial agent, 0.5-1 parts of dispersant, 0.4-0.8 parts of thickener, 0.2-0.4 parts of defoamer, and 0.05-0.1 parts of leveling agent are fully stirred to uniformly disperse to obtain an antibacterial coating;

[0010] Furthermore, the solvent is one or more of water, ethanol, isopropanol, acetone, dimethyl nylonate, propylene glycol methyl ether acetate, benzene, toluene, and xylene.

[0011] Furthermore, the filler is one or more of nano titanium dioxide, white carbon black, aluminum oxide, magnesium hydroxide, cesium tungsten bronze, and antimony tin oxide.

[0012] Furthermore, the film-forming aid is one or more of propylene glycol, propylene glycol methyl ether acetate, propylene glycol ethyl ether and propylene glycol butyl ether.

[0013] Furthermore, the antibacterial agent is prepared by the following steps:

[0014] S1. Blow a dry three-necked flask with nitrogen for 30 minutes to drive away the air in the flask, then add glycerol, 20wt% sodium hydroxide solution and chloroform, stir until completely dissolved, then slowly add epichlorohydrin, heat to 80°C after the addition is complete, stir and react for 6 hours, cool to room temperature after the reaction is completed, distill under reduced pressure, purify by column chromatography (a mixed solvent of benzene and methanol is selected as the eluent, and the volume ratio of benzene and methanol is 9:1), and distill under reduced pressure to obtain intermediate 1; the amount ratio of glycerol, epichlorohydrin, 20wt% sodium hydroxide solution and chloroform is 0.088mol:0.08mol:2.9mL:100mL;

[0015] Under heating and base catalysis conditions, the -OH of glycerol and the epoxy group of epichlorohydrin undergo a nucleophilic substitution reaction. The reaction process is as follows:

[0016]

[0017] S2. Blow nitrogen gas into a dry three-necked flask for 30 minutes to drive away the air in the flask, then add dodecyl methacrylate, DBU (1,8-diazobisspiro[5.4.0]undec-7-ene) and DMSO (dimethyl sulfoxide), stir evenly, and then slowly add bis[3-(triethoxysilane)propyl]amine. After the addition is complete, heat to 60°C and react for 18 hours. After the reaction is completed, distill under reduced pressure to obtain intermediate 2; the dosage ratio of bis[3-(triethoxysilane)propyl]amine, dodecyl methacrylate, DBU and DMSO is 39.2 g:23.4 mL:2.4 mL:180 mL;

[0018] Under the catalytic action of DBU, the molar ratio of bis[3-(triethoxysilane)propyl]amine to dodecyl methacrylate is controlled to be 1.1-1.2:1, and bis[3-(triethoxysilane)propyl]amine and dodecyl methacrylate undergo Michael addition reaction. The reaction process is as follows:

[0019]

[0020] S3. Blow nitrogen gas into a dry three-necked flask for 30 minutes to drive away the air in the flask, then add intermediate 1, triethylamine and DMSO, stir and dissolve, then slowly add a mixed solution of intermediate 2 and DMSO, heat to 80°C and react for 3 hours. After the reaction is completed, cool to room temperature and distill under reduced pressure to obtain an antibacterial agent; the dosage ratio of intermediate 1, intermediate 2, triethylamine and DMSO is 9.6 g:30.6 g:8.1 mL:180 mL.

[0021] Under the action of triethylamine, the molar ratio of intermediate 2 to intermediate 1 is controlled to be 1:1.1-1.2, and the tertiary amino group of intermediate 2 and -Cl of intermediate 1 undergo a nucleophilic substitution reaction. The reaction process is as follows:

[0022]

[0023] The antibacterial agent of the present invention is a quaternary ammonium salt antibacterial agent. The antibacterial mechanism of the quaternary ammonium salt is mainly attributed to its positive charge. These positive charges combine with the negatively charged genes on the microbial cell wall to destroy the cell wall, resulting in bacteriolysis and cell death. In addition, the quaternary ammonium salt can also denature proteins to cause cell death, destroy the semipermeability of the cell membrane, and reduce the nutrient intake for maintaining life. The mechanism of action of the quaternary ammonium salt also includes adsorption and penetration into the cell membrane, causing disorder in the cell membrane structure, causing leakage of small molecules in the cell, and then protein and nucleic acid degradation, and finally self-lytic enzymes cause cell disintegration until death. In addition, an alkyl chain in the antibacterial agent contains 15 carbons, which further increases its antibacterial effect.

[0024] The antimicrobial agent contains multiple hydroxyl groups, which can form hydrogen bonds with the carboxyl groups of the polyacrylic resin and the hydroxyl groups in the solvent. The hydrogen bonding effect allows the antimicrobial agent to be evenly dispersed in the antimicrobial coating. The antimicrobial agent also contains abundant silaneoxy groups, which hydrolyze, condense, cross-link, and form covalent bonds with the hydroxyl groups on the surface of the filler, thereby reducing the surface energy of the filler and making the filler highly dispersed in the antimicrobial coating, thereby maximizing its own effect and improving the weather resistance, antistatic properties, flame retardancy and smoke suppression of the antimicrobial coating. At the same time, it also allows the antimicrobial agent itself to stably exist in the antimicrobial coating and give full play to its antimicrobial effect.

[0025] In addition, the silaneoxy groups in the antibacterial agent can also chemically bond with the abundant hydroxyl groups on the surface of tempered glass, thereby greatly enhancing the adhesion between the antibacterial coating and the tempered glass, which further improves the stability of the antibacterial agent and filler in the antibacterial coating.

[0026] Furthermore, the dispersant is one or more of polymethoxypropyl acetate, polytrimethoxysilane, BYK201 and BYK110.

[0027] Furthermore, the thickener is a water-soluble dispersion of hydroxyacrylic acid.

[0028] Furthermore, the defoaming agent is one or more of sodium dodecyl sulfate, polyvinyl alcohol, and sodium octanoate.

[0029] Furthermore, the leveling agent is one or more of BYK358N, BYK333, and BYK301.

[0030] The present invention also discloses a tempered glass based on an antibacterial coating, and the tempered glass is prepared according to the above-mentioned method for preparing the tempered glass based on an antibacterial coating.

[0031] The beneficial effects of the present invention are as follows: the antibacterial coating has excellent adhesion to the tempered glass, the antibacterial agent containing a quaternary ammonium salt antibacterial structure in the antibacterial coating has good compatibility with other raw materials, and there is a chemical bond between the antibacterial agent and the filler. Therefore, the antibacterial agent and the filler can be highly dispersed and stably present in the antibacterial coating to fully exert their effects. Therefore, the tempered glass based on the antibacterial coating of the present invention has excellent and stable antibacterial and weather resistance properties for a long time. DETAILED DESCRIPTION

[0032] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Example 1

[0034] The preparation of the antibacterial agent comprises the following specific steps:

[0035] S1. Blow nitrogen gas into a 250 mL dry three-necked flask for 30 min to drive away the air in the flask, then add 8.1 g of glycerol, 2.9 mL of 20 wt% sodium hydroxide solution and 100 mL of chloroform, stir until completely dissolved, then slowly add 6.3 mL of epichlorohydrin, after the addition is complete, heat to 80 ° C, stir and react for 6 h, after the reaction is completed, cool to room temperature, distill under reduced pressure, purify by column chromatography, and distill under reduced pressure to obtain intermediate 1;

[0036] S2, blowing nitrogen gas into a 500 mL dry three-necked flask for 30 min to drive away the air in the flask, then adding 23.4 mL of dodecyl methacrylate, 2.4 mL of DBU and 180 mL of DMSO, stirring evenly, and then slowly adding 39.2 g of bis[3-(triethoxysilyl)propyl]amine, after the addition is complete, heating to 60 ° C to react for 18 h, after the reaction is completed, distilling under reduced pressure to obtain intermediate 2;

[0037] S3. Blow nitrogen gas into a 500mL dry three-necked flask for 30 minutes to drive away the air in the flask, then add 9.6g of intermediate 1, 8.1mL of triethylamine and 100mL of DMSO, stir to dissolve, then slowly add a mixed solution of 30.6g of intermediate 2 and 80mL of DMSO, heat to 80℃ and react for 3h. After the reaction is completed, cool to room temperature and distill under reduced pressure to obtain an antibacterial agent.

[0038] Example 2

[0039] Preparation of tempered glass, the specific steps are as follows:

[0040] (1) 40 parts of polyacrylic acid resin, 8 parts of water, 9 parts of ethanol, 9 parts of acetone, 9 parts of dimethyl nylonate, 30 parts of polyurethane resin, 5 parts of nano titanium dioxide, 5 parts of white carbon black, 5 parts of aluminum oxide, 0.5 parts of propylene glycol, 0.5 parts of propylene glycol ethyl ether, 0.5 parts of polymethoxypropyl acetate, 0.8 parts of the antibacterial agent prepared in Example 1, 0.4 parts of hydroxy acrylic acid water-soluble dispersion, 0.2 parts of sodium dodecyl sulfate, and 0.05 parts of leveling agent BYK333 were fully stirred to be uniformly dispersed, thereby preparing an antibacterial coating;

[0041] (2) The flat glass after cutting, edge grinding, washing and drying is placed in a tempering furnace and heated to 650° C., and then placed in a quenching chamber for cooling. When the temperature drops to 200° C., it is taken out and the antibacterial coating prepared in step (1) is evenly sprayed onto the glass surface. After cooling to room temperature, tempered glass based on the antibacterial coating can be prepared.

[0042] Example 3

[0043] Preparation of tempered glass, the specific steps are as follows:

[0044] (1) 48 parts of polyacrylic acid resin, 10 parts of water, 21 parts of propylene glycol methyl ether acetate, 21 parts of benzene, 37 parts of polyurethane resin, 6 parts of white carbon black, 4 parts of aluminum oxide, 4 parts of cesium tungsten bronze, 4 parts of antimony tin oxide, 2 parts of propylene glycol methyl ether acetate, 0.8 parts of BYK201, 1.1 parts of the antibacterial agent prepared in Example 1, 0.6 parts of hydroxy acrylic acid water-soluble dispersion, 0.3 parts of sodium octanoate, and 0.09 parts of leveling agent BYK358N were fully stirred to be uniformly dispersed, thereby preparing an antibacterial coating;

[0045] (2) The flat glass after cutting, edge grinding, washing and drying is placed in a tempering furnace and heated to 750° C., and then placed in a quenching chamber for cooling. When the temperature drops to 200° C., it is taken out and the antibacterial coating prepared in step (1) is evenly sprayed onto the glass surface. After cooling to room temperature, tempered glass based on the antibacterial coating can be prepared.

[0046] Example 4

[0047] Preparation of tempered glass, the specific steps are as follows:

[0048] (1) 50 parts of polyacrylic acid resin, 10 parts of water, 10 parts of ethanol, 22 parts of isopropanol, 13 parts of acetone, 40 parts of polyurethane resin, 5 parts of nano titanium dioxide, 5 parts of white carbon black, 5 parts of magnesium hydroxide, 5 parts of antimony tin oxide, 3 parts of propylene glycol butyl ether, 1 part of BYK110, 1.2 parts of the antibacterial agent prepared in Example 1, 0.8 parts of hydroxy acrylic acid water-soluble dispersion, 0.4 parts of polyvinyl alcohol, and 0.1 parts of leveling agent BYK301 were fully stirred to be uniformly dispersed, thereby preparing an antibacterial coating;

[0049] (2) The flat glass after cutting, edge grinding, washing and drying is placed in a tempering furnace and heated to 660° C., and then placed in a quenching chamber for cooling. When the temperature drops to 200° C., it is taken out and the antibacterial coating prepared in step (1) is evenly sprayed onto the glass surface. After cooling to room temperature, tempered glass based on the antibacterial coating can be prepared.

[0050] Comparative Example 1

[0051] Preparation of tempered glass, the specific steps are as follows:

[0052] The remaining steps remain unchanged, only the antibacterial agent in Example 4 is removed to prepare the tempered glass.

[0053] Comparative Example 2

[0054] Preparation of tempered glass, the specific steps are as follows:

[0055] The remaining steps remain unchanged, only the antibacterial agent in Example 4 is replaced by quaternary ammonium salt-73 to prepare tempered glass.

[0056] Performance Testing

[0057] The tempered glass prepared in Examples 2-4 and Comparative Examples 1-2 was subjected to performance tests according to the test standard specified in GB15763.2-2005 Safety Glass for Buildings. The adhesion between the antibacterial coating and the tempered glass was determined using the GB / T9286-1998 Scratching Test for Paint and Varnish Films standard. The test results are shown in Table 1 below:

[0058] Table 1

[0059]

[0060] Antibacterial properties were tested in accordance with GB / T21866-2008 "Determination of antibacterial properties and antibacterial effects of antibacterial coatings (paint films)". The test results are shown in Table 2 below:

[0061] Table 2

[0062]

[0063] “-” means no antibacterial property.

[0064] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0065] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing tempered glass based on antibacterial coating, characterized in that: The following steps are involved: 40-50 parts of polyacrylic acid resin, 35-55 parts of solvent, 30-40 parts of polyurethane resin, 15-20 parts of filler, 1-3 parts of film-forming aid, 0.8-1.2 parts of antibacterial agent, 0.5-1 parts of dispersant, 0.4-0.8 parts of thickener, 0.2-0.4 parts of defoamer, and 0.05-0.1 parts of leveling agent are fully stirred to disperse evenly to obtain antibacterial coating; the flat glass after cutting, edge grinding, washing and drying is placed in a tempering furnace and heated to 650-750°C, and when cooled to 200°C, it is taken out, and the antibacterial coating is sprayed on the glass surface, and cooled to room temperature to obtain tempered glass; Wherein, the antibacterial agent is prepared by the following steps: S1, after nitrogen blowing into the flask, add glycerol, 20wt% sodium hydroxide solution and chloroform, stir, add epichlorohydrin, react at 80℃ for 6h, cool, distill under reduced pressure, purify by column chromatography, and distill under reduced pressure to obtain intermediate 1; S2, after nitrogen blowing into the flask, add dodecyl methacrylate, DBU and DMSO, stir, add bis[3-(triethoxysilyl)propyl]amine, react at 60°C for 18h, and distill under reduced pressure to obtain intermediate 2; S3. After nitrogen is blown into the flask, intermediate 1, triethylamine and DMSO are added, stirred, intermediate 2 and DMSO are added, reacted at 80° C. for 3 h, cooled, and distilled under reduced pressure to obtain an antibacterial agent.

2. The method for preparing tempered glass based on antibacterial coating according to claim 1, characterized in that: The amount ratio of glycerol, epichlorohydrin, 20wt% sodium hydroxide solution and chloroform in step S1 is 0.088mol:0.08mol:2.9mL:100mL; the amount ratio of bis[3-(triethoxysilyl)propyl]amine, dodecyl methacrylate, DBU and DMSO in step S2 is 39.2g:23.4mL:2.4mL:180mL; the amount ratio of intermediate 1, intermediate 2, triethylamine and DMSO in step S3 is 9.6g:30.6g:8.1mL:180mL.

3. The method for preparing tempered glass based on antibacterial coating according to claim 1, characterized in that: The solvent is one or more of water, ethanol, isopropanol, acetone, dimethyl nylonate, propylene glycol methyl ether acetate, benzene, toluene and xylene.

4. The method for preparing tempered glass based on antibacterial coating according to claim 1, characterized in that: The filler is one or more of nano titanium dioxide, white carbon black, aluminum oxide, magnesium hydroxide, cesium tungsten bronze, and antimony tin oxide.

5. The method for preparing tempered glass based on antibacterial coating according to claim 1, characterized in that: The film-forming aid is one or more of propylene glycol, propylene glycol methyl ether acetate, propylene glycol ethyl ether and propylene glycol butyl ether.

6. The method for preparing tempered glass based on antibacterial coating according to claim 1, characterized in that: The dispersant is one or more of polymethoxypropyl acetate, polytrimethoxysilane, BYK201 and BYK110.

7. The method for preparing tempered glass based on antibacterial coating according to claim 1, characterized in that: The thickener is a water-soluble dispersion of hydroxy acrylic acid.

8. The method for preparing tempered glass based on antibacterial coating according to claim 1, characterized in that: The defoaming agent is one or more of sodium dodecyl sulfate, polyvinyl alcohol and sodium octanoate.

9. The method for preparing tempered glass based on antibacterial coating according to claim 1, characterized in that: The leveling agent is one or more of BYK358N, BYK333 and BYK301.

10. A tempered glass based on an antibacterial coating, characterized in that: The tempered glass is prepared according to the method for preparing an antibacterial coating according to any one of claims 1 to 9.

Citation Information

Cited By

  • Super anti-pollution soft light brick and preparation method thereof

    CN119409479A