Fiber-reinforced polymer protective coating with corrosion inhibition effect as well as preparation method and application of fiber-reinforced polymer protective coating
By functionalizing the fibers and growing nanomaterials, a modified fiber and resin composite material is formed, and a fiber-reinforced polymer protective coating with corrosion inhibition is prepared, which solves the interface failure of carbon fiber-reinforced composite materials in extreme marine environments and Corrosion problems significantly improve protection performance and life.
Patent Information
- Application Number
- CN202310596378.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
Existing carbon fiber reinforced composite materials are prone to interface failure in extreme marine environments, resulting in reduced impact resistance and increased permeability rate of corrosive media under deep-sea high pressure, seriously reducing protective performance.
By performing surface functionalization of the fibers and growing functional nanomaterials in situ on their surface, forming modified fibers, combining resins and curing agents, a fiber-reinforced polymer protective coating with corrosion inhibition is prepared to enhance the fibers and resins. The interface compatibility and density enhance the mechanical and erosion resistance of the protective coating.
It significantly improves the anti-erosion wear and corrosion performance of the fiber-reinforced polymer protective coating, and can effectively resist corrosion, erosion wear and external impact in extreme marine environments, and extends the service life of metal materials.
Smart Images

Figure CN119019908A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field, and in particular relates to a fiber-reinforced polymer protective coating with corrosion inhibition effect and a preparation method and application thereof. Background Art
[0002] The marine environment is characterized by high salt, high temperature, and high humidity, which can easily cause serious corrosion damage to metal materials, thereby reducing the service life and safety and reliability of marine engineering equipment. Therefore, the importance of developing long-lasting marine protective materials in the field of metal corrosion protection is self-evident. Unlike ordinary marine environments, the hydrostatic high pressure in deep-sea environments not only tests the impact resistance of protective materials, but also promotes the diffusion of corrosive media in protective materials, thereby accelerating the damage and failure of protective materials. At the same time, with my country's scientific exploration of the 10,000-meter deep sea and the future demand for deep-sea resource drilling, deep-sea engineering equipment has put forward new requirements and challenges for the service performance of deep-sea protective materials. Among many protective materials, carbon fiber reinforced composite materials, with their excellent mechanical properties, chemical stability, corrosion resistance and impact resistance, have shown great application potential in the field of corrosion protection of metal materials in marine environments. However, the surface of untreated carbon fiber is smooth and has few active functional groups, which makes carbon fiber reinforced composites prone to interface failure under the action of multiple factors in extreme environments, and forms stress concentration in the interface area of carbon fiber / resin matrix, which greatly reduces the impact resistance of the composite material, seriously restricting the high performance of carbon fiber reinforced composites. In particular, the high pressure in deep-sea environment can significantly increase the penetration rate of corrosive media and promote the evolution of internal defects of carbon fiber reinforced composites into microcracks, so that corrosion products accumulate at the metal / protective material interface, greatly reducing the protective performance of carbon fiber reinforced composites. Therefore, designing and developing high-performance and long-term protective carbon fiber reinforced composites is an important topic of current research. At present, most of the research focuses on constructing a new interface layer on the fiber surface through surface modification to improve the interface performance of fiber reinforced composites. However, on the one hand, the new interface layer has limited improvement on the interface performance of the composite material, and it is still difficult to meet the service requirements in the extreme environment of deep-sea high pressure; on the other hand, the prepared protective material only passively improves its protective performance by increasing its density, and its corrosion resistance is still not ideal. Therefore, it is urgent to design and develop carbon fiber reinforced composite materials with strong interface bonding and corrosion inhibition to meet their excellent mechanical properties, corrosion resistance, erosion resistance and deep-sea high-pressure resistance in extreme deep-sea service environments. Summary of the invention
[0003] The main purpose of the present invention is to provide a fiber-reinforced polymer protective coating with corrosion inhibition effect and a preparation method and application thereof, so as to overcome the shortcomings of the prior art.
[0004] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0005] The embodiment of the present invention provides a method for preparing a fiber-reinforced polymer protective coating having a corrosion inhibition effect, which comprises:
[0006] Performing surface functionalization treatment on the fiber, and then in-situ growing functional nanomaterials on the surface of the obtained fiber to obtain modified fiber;
[0007] The modified fiber is mixed and dispersed evenly with a resin and a curing agent to obtain a resin-based fiber composite material;
[0008] Furthermore, the resin-based fiber composite material is applied to the surface of a metal substrate and cured to obtain a fiber-reinforced polymer protective coating with corrosion inhibition effect.
[0009] The embodiment of the present invention also provides a fiber-reinforced polymer protective coating with corrosion inhibition effect obtained by the aforementioned preparation method.
[0010] The embodiment of the present invention also provides the application of the aforementioned fiber-reinforced polymer protective coating with corrosion inhibition in the field of metal material protection of marine engineering equipment serving in extreme marine environments.
[0011] Compared with the prior art, the present invention has the following beneficial effects:
[0012] (1) The fiber-reinforced polymer protective coating of the present invention is coated on the surface of the metal material substrate by resin, and the fiber powder filler in the resin is modified by in-situ growth of functional nanoparticles to achieve the purpose of surface modification. The modification not only greatly improves the interface compatibility and interface shear strength between the fiber and the resin, but also improves the density of the protective coating;
[0013] (2) The fiber-reinforced polymer protective coating of the present invention has excellent mechanical properties and impact resistance. At the same time, the strong interface bonding between the functional nanoparticles and the resin matrix improves the density and mechanical strength of the composite coating. In addition, the metal cations of the nanoparticles themselves have a certain corrosion inhibition effect, which can effectively slow down the corrosion rate of the metal material matrix and improve the corrosion resistance of the composite protective coating. Therefore, under the synergistic effect of the above-mentioned fibers and functional nanoparticles, the fiber-reinforced polymer protective coating has both excellent erosion and wear resistance and corrosion resistance, and can effectively resist the corrosion, erosion and wear and external force impact damage to the surface of the metal material matrix caused by the complex and harsh extreme marine environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0015] Figure 1 This is a surface optical photograph of the protective coating prepared in Example 1 of the present invention;
[0016] Figure 2 This is an optical photograph of the surface of the protective coating after erosion and wear obtained in Example 1 of the present invention;
[0017] Figure 3- Figure 3b The three-dimensional morphology of the surface of the protective coating after erosion and wear obtained in Example 1 of the present invention and Comparative Example 3;
[0018] Figure 4 This is a comparison diagram of electrochemical impedance curves of the protective coating prepared in Example 1 of the present invention and the protective coating prepared in Comparative Examples 1-3 under the action of alternating pressure;
[0019] Figure 5 1 is a comparison diagram of the tensile stress-strain curves of the protective coating prepared in Example 1 of the present invention and the protective coating prepared in Comparative Examples 1-3. DETAILED DESCRIPTION
[0020] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Specifically, as one aspect of the technical solution of the present invention, a method for preparing a fiber-reinforced polymer protective coating with corrosion inhibition comprises:
[0022] Performing surface functionalization treatment on the fiber, and then in-situ growing functional nanomaterials on the surface of the obtained fiber to obtain modified fiber;
[0023] The modified fiber is mixed and dispersed evenly with a resin and a curing agent to obtain a resin-based fiber composite material;
[0024] Furthermore, the resin-based fiber composite material is applied to the surface of a metal substrate and cured to obtain a fiber-reinforced polymer protective coating with corrosion inhibition effect.
[0025] The present invention constructs an interface reinforcement layer with excellent bonding force between the fiber and the resin, improves the interface performance between the resin substrate and the filler, and enhances the mechanical properties of the protective coating. At the same time, the functional nanoparticles give the protective coating an excellent corrosion inhibition effect, so that the protective coating has high erosion and wear resistance and corrosion resistance, and can effectively resist corrosion, erosion and wear, and external force impact damage to the surface of the metal material substrate caused by the complex and harsh marine environment.
[0026] In some preferred embodiments, the fiber includes any one of carbon fiber, basalt fiber, aramid fiber, polyimide fiber, and glass fiber, or a combination of two or more thereof, and is not limited thereto.
[0027] In some preferred embodiments, the fiber has a diameter of 3-15 μm and a length of 10-500 μm.
[0028] In some preferred embodiments, the functional nanomaterial includes any one or a combination of two or more of cerium-imidazole framework structure nanoparticles, zinc-imidazole framework structure nanoparticles, and cerium dioxide nanoparticles, and is not limited thereto.
[0029] In some preferred embodiments, the preparation method specifically includes: using a strong oxidizing acid and performing surface functionalization treatment on the fiber at 60-150° C., wherein the surface functionalization treatment at least introduces carboxyl functional groups and / or hydroxyl functional groups into the surface of the obtained fiber.
[0030] Furthermore, the strong oxidizing acid includes any one of sulfuric acid, nitric acid, and hypochlorous acid, or a combination of two or more thereof, but is not limited thereto.
[0031] In some preferred embodiments, the preparation method specifically comprises: placing the fiber obtained by surface functionalization treatment in a solution containing metal cations, then adding a solution containing anionic ligands and stirring the reaction at 25-60° C. to obtain the modified fiber.
[0032] Furthermore, the metal cation includes any one of cerium ion, zinc ion, copper ion or a combination of two or more thereof, but is not limited thereto.
[0033] Furthermore, the anionic ligand includes any one of imidazolate, carboxylate, and phenolic acid ester or a combination of two or more thereof, but is not limited thereto.
[0034] In some preferred embodiments, the preparation method specifically includes: mixing and dispersing the modified fiber and resin evenly, and then adding a curing agent to mix to form the resin-based fiber composite material; wherein the mass ratio of the modified fiber to the resin is 0.5-10:100.
[0035] Furthermore, the resin includes any one of epoxy resin, acrylic resin, silicone resin, and phenolic resin, or a combination of two or more thereof, but is not limited thereto.
[0036] Furthermore, the curing agent includes any one or a combination of two or more of an amine curing agent, an acid anhydride curing agent, a sulfonic acid curing agent, and an azo curing agent, but is not limited thereto.
[0037] In some preferred embodiments, the preparation method further comprises: first placing the resin-based fiber composite material in a vacuum environment for 5-10 minutes, at least to remove gas in the resin-based fiber composite material.
[0038] In some preferred embodiments, the preparation method specifically comprises: applying the resin-based fiber composite material to the surface of a metal substrate, and curing it at 25-100° C. for 4-36 hours.
[0039] Furthermore, the resin-based fiber composite material is applied to the surface of the metal substrate and cured at 25° C. for 12 h, 40° C. for 12 h, 60° C. for 2 h, and 80° C. for 2 h.
[0040] In some more specific embodiments, the method for preparing the fiber-reinforced polymer protective coating having a corrosion inhibition effect comprises:
[0041] Add the fiber powder modified with the surface of functional nanomaterials (i.e. the aforementioned "modified fiber") into the resin and stir to obtain a uniformly dispersed slurry;
[0042] Adding a curing agent to the slurry and mixing them evenly to obtain a resin-based fiber composite material, and then placing the resin-based fiber composite material in a vacuum environment and evacuating it for 5-10 minutes;
[0043] Applying the resin-based fiber composite material to the surface of the metal material substrate to form a protective coating;
[0044] The protective coating is cured by curing at elevated temperatures to obtain a fiber-reinforced polymer protective coating with corrosion inhibition effect.
[0045] Furthermore, the surface modification method of the fiber is: using a strong oxidizing acid to perform surface functionalization treatment on the fiber under high temperature conditions, introducing carboxyl groups and hydroxyl groups on the fiber surface to improve the reaction activity of the fiber, and then in situ growing functional nanomaterials on the surface of the functionalized fiber.
[0046] Furthermore, the strong oxidizing acid includes at least one of sulfuric acid, nitric acid, hypochlorous acid, or a combination of two or more thereof.
[0047] Furthermore, the high temperature range is 60-150°C.
[0048] Furthermore, the in-situ growth process of the functional nanomaterial is as follows: (1) preparing a relevant metal cation solution, and adding the fiber with surface functionalization treatment to the solution, and stirring at a constant temperature and high speed; (2) preparing a relevant anion ligand solution, and adding the anion ligand solution dropwise to the metal cation solution of step (1), and stirring at a constant temperature and high speed; (3) after continuing to stir at a constant temperature and high speed for a certain period of time, the obtained solution is centrifuged, washed and dried, and the obtained solution is a fiber powder with surface modification of the functionalized nanomaterial.
[0049] Wherein, the metal cations include at least one of cerium ions and zinc ions or a combination of two or more thereof.
[0050] The temperature-increasing curing method includes: curing at 25° C. and 40° C. for 12 hours, respectively, and then curing at 60° C. and 80° C. for 2 hours, respectively.
[0051] Another aspect of the embodiments of the present invention further provides a fiber-reinforced polymer protective coating with corrosion inhibition effect obtained by the aforementioned preparation method.
[0052] Furthermore, the fiber-reinforced polymer protective coating has a thickness of 100 μm-1000 μm.
[0053] Furthermore, after the fiber-reinforced polymer protective coating was immersed in alternating hydrostatic pressure for 168 hours, its coating impedance was still as high as 9.37×10 8 Ω·cm 2 Under continuous scouring of high-sand-content, high-velocity mud, the coating mass loss and volume loss were reduced by 31.68% and 24.78% respectively compared with pure epoxy coating.
[0054] Specifically, the fiber-reinforced polymer protective coating is coated on the surface of a metal material substrate, with a resin material as the matrix, and the modified fiber powder is added to the resin for curing and forming, wherein the fiber is functionally surface modified, and nanomaterials with corrosion inhibition function grow on the fiber surface, and the modified fiber-reinforced polymer coating has corrosion inhibition, wave absorption, heat conduction, and anti-erosion, wear and corrosion resistance.
[0055] Another aspect of the embodiments of the present invention further provides the application of the aforementioned fiber-reinforced polymer protective coating with corrosion inhibition in the field of metal material protection of marine engineering equipment serving in extreme marine environments.
[0056] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0057] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.
[0058] Example 1
[0059] (1) Carbon fiber pretreatment
[0060] 1.0 g of original carbon fiber was added into 2 mol / L sodium hydroxide solution, stirred and reacted at 80 °C for 4 h, and then washed with deionized water until neutral;
[0061] The carbon fiber was then added to acetone, refluxed and stirred at 60° C. for 4 h, then washed with deionized water, and dried in a vacuum drying oven at 50° C. for 24 h to obtain pretreated carbon fiber.
[0062] (2) Oxidation treatment of carbon fiber
[0063] 1.0 g of the pretreated carbon fiber was added to 50 mL of nitric acid, stirred and reacted at 90° C. for 6 h, then washed with deionized water until neutral, and dried in a vacuum drying oven at 50° C. for 24 h to obtain oxidized carbon fiber.
[0064] (3) Carbon fiber surface modification
[0065] Take 0.2 g of cerium nitrate hexahydrate and dissolve it in 50 mL of methanol, then take 1.0 g of 2-methylimidazole and dissolve it in 50 mL of methanol;
[0066] 0.4 g of oxidized carbon fiber was added to the cerium nitrate-methanol solution, and stirred at 1500 r / min for 30 min at 25 °C. Then, the imidazole-methanol solution was added dropwise to the cerium nitrate-methanol solution, and the stirring was continued for 3 h under the original conditions.
[0067] After the reaction is completed, the mixture is centrifuged at 10000 r / min for 10 min and the precipitate is retained. The sample is then centrifuged and washed three times at 10000 r / min using methanol and dried in a vacuum drying oven at 50° C. for 24 h to obtain modified carbon fiber.
[0068] (4) Preparation of protective coating
[0069] Adding 5 wt% of modified carbon fiber into epoxy resin and stirring at high speed to obtain a mixed slurry of modified carbon fiber and epoxy resin;
[0070] Adding epoxy resin curing agent into the mixed slurry and mixing evenly to obtain a modified carbon fiber / polymer composite coating, wherein the mass ratio of the curing agent to the epoxy resin is 60:100;
[0071] The composite coating is coated on the surface of the metal material substrate, and is cured at 25°C and 40°C for 12 hours respectively, and then cured at 60°C and 80°C for 2 hours respectively, to obtain the above-mentioned carbon fiber reinforced polymer protective coating with corrosion inhibition effect.
[0072] As shown in FIG1, it is a surface optical photograph of the carbon fiber reinforced polymer protective coating prepared in this embodiment. It can be seen that there is no bubbling and separation inside the carbon fiber reinforced polymer protective coating, and the coating surface is smooth and flat without defects such as pores and cracks. This indicates that the interface between the fiber filler and the resin in the coating and between the coating and the metal substrate is well bonded, which also lays a good foundation for the protective coating to have excellent anti-erosion, wear and corrosion protection performance in the subsequent service process.
[0073] like Figure 2 As shown, it is an optical photograph of the eroded surface of the carbon fiber reinforced polymer protective coating prepared in this embodiment after the surface was eroded at a speed of 3.13m / s in a silicon carbide aqueous solution (silicon carbide mass fraction 20wt%) for 30 minutes; it can be seen that the surface appearance of the carbon fiber reinforced polymer protective coating is good, without obvious cracks, and the volume loss and mass loss after erosion are very small, indicating that the protective coating can resist the impact of high-intensity sand and gravel water flow, and the protective coating has excellent resistance to long-term erosion and wear. This is mainly due to the significant improvement of the interface performance between the modified carbon fiber and the resin, wherein the interface performance includes interface compatibility and interface shear strength.
[0074] Furthermore, if Figure 3a , Figure 3b As shown, the three-dimensional morphology of the surface of the carbon fiber reinforced polymer protective coating after erosion obtained in this embodiment and comparative example 3 respectively; it can be seen that the internal depth of the erosion pits on the surface of the protective coating obtained in this embodiment decreases evenly, and there is no obvious local peeling phenomenon, and the depth of the erosion pits is only 1.16 mm, which is much lower than the protective coating obtained in comparative example 3, indicating that the protective coating in this embodiment has excellent performance in resisting erosion and wear.
[0075] like Figure 4As shown, the initial electrical impedance curves of the carbon fiber reinforced polymer protective coating prepared in this embodiment and the protective coating prepared in comparative example 1, as well as the comparison of the electrical impedance curves of the two after 7 cycles of alternating pressure. Among them, one cycle includes 12 hours of high hydrostatic pressure immersion (20MPa) and 12 hours of normal pressure immersion (0.1MPa). In the figure, the horizontal axis represents frequency (frequency), the unit is Hertz (Hz), and the vertical axis represents impedance, the unit is Ohm (Ohm), and the frequency and impedance are expressed in logarithmic form. It can be seen that the initial electrical impedance curves of the two coatings are not significantly different, and after 7 cycles of alternating pressure, the low-frequency impedance values of the two have dropped significantly, but the protective coating in this embodiment still has a higher impedance modulus at low frequencies, and its low-frequency impedance value can reach 9.8×10 8 Ω / cm 2 , while the low-frequency impedance value of the protective coating in comparative example 1 is only 2.9×10 6 Ω / cm 2 . It shows that the modified carbon fiber can improve the density of the coating, and give the coating excellent high pressure resistance and resistance to penetration of corrosive media. At the same time, the cerium-imidazole skeleton structure on the surface of the modified carbon fiber can provide cerium ions with corrosion inhibition, further delaying the corrosion process of the metal substrate. Therefore, the protective coating in this embodiment has excellent corrosion protection performance.
[0076] like Figure 5 As shown, it is a comparison diagram of the tensile stress-strain curves of the carbon fiber reinforced polymer protective coating prepared in this embodiment and the protective coating prepared in comparative examples 1-3. In the figure, the abscissa represents strain in %, and the ordinate represents stress in MPa. It can be seen that although the tensile strain of the protective coating in comparative example 2 increases significantly, the tensile stress decreases significantly. In this embodiment, the tensile stress and tensile strain of the carbon fiber reinforced polymer protective coating both increase significantly, indicating that the mechanical properties and toughness of the protective coating are significantly improved, and at the same time, the erosion resistance and corrosion resistance of the carbon fiber reinforced polymer protective coating are indirectly improved.
[0077] Example 2
[0078] (1) Glass fiber pretreatment
[0079] 1.0 g of original glass fiber was added into 2 mol / L sodium hydroxide solution, stirred at 80 °C for 4 h, and then washed with deionized water until neutral;
[0080] The glass fiber was then added to acetone, refluxed and stirred at 60° C. for 4 h, then washed with deionized water, and dried in a vacuum drying oven at 50° C. for 24 h to obtain the pretreated glass fiber.
[0081] (2) Glass fiber oxidation treatment
[0082] 1.0 g of the pretreated glass fiber was added to 50 mL of nitric acid, stirred and reacted at 90° C. for 6 h, then washed with deionized water until neutral, and dried in a vacuum drying oven at 50° C. for 24 h to obtain oxidized glass fiber.
[0083] (3) Surface modification of glass fiber
[0084] 0.4 g of oxidized glass fiber was added to 0.08 mol / L cerium nitrate aqueous solution, and stirred at 1500 r / min for 30 min at 25 °C. Then 3 mol / L ammonia water was added dropwise to the cerium nitrate aqueous solution until pH = 10, and stirring was continued for 3 h under the original conditions;
[0085] After the reaction was completed, the mixture was centrifuged at 10000 r / min for 10 min and the precipitate was retained. The sample was then centrifuged and washed three times at 10000 r / min using methanol and dried in a vacuum drying oven at 50° C. for 24 h to obtain modified glass fiber.
[0086] (4) Preparation of protective coating
[0087] Adding 5 wt% of modified glass fiber into epoxy resin and stirring at high speed to obtain a mixed slurry of modified glass fiber and epoxy resin;
[0088] Adding epoxy resin curing agent into the mixed slurry and mixing evenly to obtain a modified glass fiber / polymer composite coating, wherein the mass ratio of the curing agent to the epoxy resin is 60:100;
[0089] The composite coating is coated on the surface of the metal material substrate, and cured at 25°C and 40°C for 12 hours respectively, and then cured at 60°C and 80°C for 2 hours respectively, to obtain the above-mentioned glass fiber reinforced polymer protective coating with corrosion inhibition effect.
[0090] In this embodiment, the fiber-reinforced coating has excellent erosion resistance and mechanical properties, and its low-frequency impedance value can still reach 8.9×10 8 Ω / cm 2 .
[0091] Example 3
[0092] (1) Basalt fiber pretreatment
[0093] 1.0 g of original basalt fiber was added into 2 mol / L sodium hydroxide solution, stirred and reacted at 80 °C for 4 h, and then washed with deionized water until neutral;
[0094] The basalt fiber was then added to acetone, refluxed and stirred at 60° C. for 4 h, then washed with deionized water, and dried in a vacuum drying oven at 50° C. for 24 h to obtain the pretreated basalt fiber.
[0095] (2) Oxidation treatment of basalt fiber
[0096] 1.0 g of the pretreated basalt fiber was added to 50 mL of nitric acid, stirred and reacted at 90° C. for 6 h, then washed with deionized water until neutral, and dried in a vacuum drying oven at 50° C. for 24 h to obtain oxidized basalt fiber.
[0097] (3) Surface modification of basalt fiber
[0098] Take 0.2 g of zinc nitrate hexahydrate and dissolve it in 20 mL of methanol, then take 0.5 g of 2-methylimidazole and dissolve it in 20 mL of methanol;
[0099] 0.4 g of oxidized basalt fiber was added to 30 mL of methanol and stirred at 1500 r / min at 25 °C. Then, zinc nitrate-methanol solution was added dropwise to the basalt fiber-methanol mixture and stirred continuously for 1 h.
[0100] Add the imidazole-methanol solution to the mixed solution and continue stirring for 5 h under the original conditions;
[0101] After the reaction was completed, the mixture was centrifuged at 10000 r / min for 10 min and the precipitate was retained. The sample was then centrifuged and washed three times at 10000 r / min using methanol and dried in a vacuum drying oven at 50° C. for 24 h to obtain modified basalt fiber.
[0102] (4) Preparation of protective coating
[0103] Adding 5 wt% of modified basalt fiber into epoxy resin and stirring at high speed to obtain a mixed slurry of modified basalt fiber and epoxy resin;
[0104] Adding epoxy resin curing agent into the mixed slurry and mixing evenly to obtain a modified basalt fiber / polymer composite coating, wherein the mass ratio of the curing agent to the epoxy resin is 60:100;
[0105] The composite coating is coated on the surface of the metal material substrate, and is cured at 25°C and 40°C for 12 hours respectively, and then cured at 60°C and 80°C for 2 hours respectively, to obtain the above-mentioned basalt fiber reinforced polymer protective coating with corrosion inhibition effect.
[0106] In this embodiment, the fiber-reinforced coating has excellent erosion resistance and mechanical properties, and its low-frequency impedance value can still reach 8.31×10 8Ω / cm 2 .
[0107] Comparative Example 1
[0108] Adding epoxy resin curing agent into epoxy resin and mixing them evenly to obtain polymer coating, wherein the mass ratio of curing agent to epoxy resin is 60:100;
[0109] The polymer coating is coated on the surface of the metal material substrate, and is cured at 25°C and 40°C for 12 hours respectively, and then cured at 60°C and 80°C for 2 hours respectively, to obtain a polymer protective coating.
[0110] Comparative Example 2
[0111] (1) Carbon fiber pretreatment
[0112] 1.0 g of original carbon fiber was added into 2 mol / L sodium hydroxide solution, stirred and reacted at 80 °C for 4 h, and then washed with deionized water until neutral;
[0113] The carbon fiber was then added to acetone, refluxed and stirred at 60° C. for 4 h, then washed with deionized water, and dried in a vacuum drying oven at 50° C. for 24 h to obtain pretreated carbon fiber.
[0114] (2) Oxidation treatment of carbon fiber
[0115] 1.0 g of the pretreated carbon fiber was added to 50 mL of nitric acid, stirred and reacted at 90° C. for 6 h, then washed with deionized water until neutral, and dried in a vacuum drying oven at 50° C. for 24 h to obtain oxidized carbon fiber.
[0116] (3) Preparation of protective coating
[0117] A mixture of oxidized carbon fibers and cerium-imidazole framework structure nanoparticles with a mass fraction of 5 wt % (the ratio of the two being the same as in Example 1) is added to epoxy resin and stirred at high speed to obtain a mixed slurry;
[0118] Adding epoxy resin curing agent into the mixed slurry and mixing evenly to obtain a composite coating, wherein the mass ratio of the curing agent to the epoxy resin is 60:100;
[0119] The composite coating is coated on the surface of the metal material substrate, and is cured at 25°C and 40°C for 12 hours respectively, and then cured at 60°C and 80°C for 2 hours respectively, to obtain a polymer protective coating.
[0120] Comparative Example 3
[0121] (1) Carbon fiber pretreatment
[0122] 1.0 g of original carbon fiber was added into 2 mol / L sodium hydroxide solution, stirred and reacted at 80 °C for 4 h, and then washed with deionized water until neutral;
[0123] The carbon fiber was then added to acetone, refluxed and stirred at 60° C. for 4 h, then washed with deionized water, and dried in a vacuum drying oven at 50° C. for 24 h to obtain pretreated carbon fiber.
[0124] (2) Oxidation treatment of carbon fiber
[0125] 1.0 g of the pretreated carbon fiber was added to 50 mL of nitric acid, stirred and reacted at 90° C. for 6 h, then washed with deionized water until neutral, and dried in a vacuum drying oven at 50° C. for 24 h to obtain oxidized carbon fiber.
[0126] (3) Preparation of protective coating
[0127] Adding 5 wt% of oxidized carbon fiber into epoxy resin and stirring at high speed to obtain a mixed slurry;
[0128] Adding epoxy resin curing agent into the mixed slurry and mixing evenly to obtain a composite coating, wherein the mass ratio of the curing agent to the epoxy resin is 60:100;
[0129] The composite coating is coated on the surface of the metal material substrate, and is cured at 25°C and 40°C for 12 hours respectively, and then cured at 60°C and 80°C for 2 hours respectively, to obtain a polymer protective coating.
[0130] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0131] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. A method for preparing a fiber-reinforced polymer protective coating with corrosion inhibition, characterized in that: include: Performing surface functionalization treatment on the fiber, and then in-situ growing functional nanomaterials on the surface of the obtained fiber to obtain modified fiber; The modified fiber is mixed and dispersed evenly with a resin and a curing agent to obtain a resin-based fiber composite material; Furthermore, the resin-based fiber composite material is applied to the surface of a metal substrate and cured to obtain a fiber-reinforced polymer protective coating with corrosion inhibition effect.
2. The preparation method according to claim 1, characterized in that: The fiber includes any one of carbon fiber, basalt fiber, aramid fiber, polyimide fiber, and glass fiber, or a combination of two or more thereof; and / or, the fiber has a diameter of 3-15 μm and a length of 10-500 μm; And / or, the functional nanomaterial includes any one of cerium-imidazole framework structure nanoparticles, zinc-imidazole framework structure nanoparticles, and cerium dioxide nanoparticles, or a combination of two or more thereof.
3. The preparation method according to claim 1, characterized in that Specifically include: The fiber is subjected to surface functionalization treatment at 60-150° C. using a strong oxidizing acid, wherein the surface functionalization treatment at least introduces carboxyl functional groups and / or hydroxyl functional groups into the surface of the obtained fiber; preferably, the strong oxidizing acid comprises any one of sulfuric acid, nitric acid, and hypochlorous acid, or a combination of two or more thereof.
4. The preparation method according to claim 1, characterized in that Specifically include: The fiber obtained by the surface functionalization treatment is placed in a solution containing metal cations, and then a solution containing anionic ligands is added and stirred for reaction at 25-60° C. to obtain the modified fiber.
5. The preparation method according to claim 4, characterized in that: The metal cations include any one of cerium ions, zinc ions, and copper ions, or a combination of two or more thereof; And / or, the anionic ligand includes any one of imidazolate, carboxylate, and phenolic acid ester, or a combination of two or more thereof.
6. The preparation method according to claim 1, characterized in that Specifically include: The modified fiber and the resin are mixed and dispersed uniformly, and then a curing agent is added and mixed to form the resin-based fiber composite material; wherein the mass ratio of the modified fiber to the resin is 0.5-10:100; Preferably, the resin includes any one of epoxy resin, acrylic resin, silicone resin, and phenolic resin, or a combination of two or more thereof; preferably, the curing agent includes any one of amine curing agents, anhydride curing agents, sulfonic acid curing agents, and azo curing agents, or a combination of two or more thereof.
7. The preparation method according to claim 1, characterized in that Also includes: The resin-based fiber composite material is first placed in a vacuum environment for 5-10 minutes, at least to remove gas in the resin-based fiber composite material.
8. The preparation method according to claim 1, characterized in that Specifically include: The resin-based fiber composite material is applied to the surface of a metal substrate and cured at 25-100° C. for 4-36 hours.
9. A fiber-reinforced polymer protective coating with corrosion inhibition effect obtained by the preparation method according to any one of claims 1 to 8; preferably, the fiber-reinforced polymer protective coating has a thickness of 100 μm-1000 μm.
10. Use of the fiber-reinforced polymer protective coating with corrosion inhibition as claimed in claim 9 in the field of metal material protection of marine engineering equipment serving in extreme marine environments.
Citation Information
Patent Citations
Multi-scale carbon fiber, reinforced toughened epoxy composite and their preparation methods
CN110714330A
Preparation method of high-corrosion-resistance modified epoxy resin composite coating
CN112341900A