Elastic adhesive, combined product for road seal, anti-skid road seal structure and preparation method and application of anti-skid road seal structure

By using high-performance emulsified asphalt combined with modified asphalt and anti-slip particles, the problem of weak performance of traditional sealing cementing materials is solved, better bonding performance and durability are achieved, and the anti-slip and resistance of road sealing is improved. Grinding performance.

CN119019980APending Publication Date: 2024-11-26GUANGDONG HUALU TRANSPORTATION TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411134336.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In traditional road sealing technology, the comprehensive performance of commercially available emulsified asphalt or modified emulsified asphalt as cementitious materials is weak, resulting in problems such as peeling and granulation removal in the early stage of the sealing layer, which limits the promotion and application of sealing maintenance technology.

Method used

Adopt an elasticity including petroleum asphalt, water, acid, emulsifier, stabilizing additive, viscoelastic additive, compatibility agent, anti-aging agent, polyurethane block copolymer emulsion and sulfide silane coupling agent The adhesive, through the mixing of modified bitumen and soap liquid, forms high-performance emulsified bitumen, and combines with anti-slip particles and reactive cover agent to build an anti-slip road seal structure.

Benefits of technology

It improves the bonding performance, aging resistance and thermal oxygen aging resistance of the seal, extends the service life of the seal, enhances the anti-slip performance and wear resistance, and reduces the wear loss rate after high temperature or ultraviolet aging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019980A_ABST
    Figure CN119019980A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of road maintenance, and particularly relates to an elastic adhesive, a combined product for a road seal, an anti-skid road seal structure as well as a preparation method and application of the anti-skid road seal structure. The elastic adhesive is prepared from the following raw materials in percentage by mass: 45 to 55 percent of petroleum asphalt, 30 to 40 percent of water, 0.9 to 1.2 percent of acid, 0.8 to 1.2 percent of emulsifier, 0.4 to 1 percent of stabilizing aid, 3 to 5 percent of viscoelastic aid, 2 to 3 percent of compatilizer, 0.5 to 0.8 percent of anti-aging agent, 5 to 6 percent of polyurethane block copolymer emulsion and 0.2 to 0.3 percent of sulfide silane coupling agent. The elastic adhesive provided by the invention is high-performance emulsified asphalt which is fast in demulsification, excellent in adhesive performance and resistant to aging, the viscoelastic auxiliary agent is combined with the polyurethane block copolymer emulsion for composite modification, and the elastic adhesive has higher adhesive strength and elastic recovery capability, and can strongly connect anti-skid particles and improve the comprehensive performance of a sand seal layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of road maintenance, and in particular relates to an elastic adhesive, a combination product for road sealing, an anti-skid road sealing structure, and a preparation method and application thereof. Background Art

[0002] In recent years, highway traffic has developed rapidly, the scale of highway construction has continued to maintain a high level, and the total mileage of highways has increased year by year. Generally speaking, the service level of highways during operation will continue to decrease as the service time increases, mainly manifested in: (1) the surface texture of aggregates is worn away under the repeated action of wheel loads, and the anti-skid performance is sharply reduced. (2) The surface mixture ages, micro cracks appear, and surface water seeps into the road, endangering the pavement structure.

[0003] At present, widely used preventive maintenance measures to improve skid resistance include: hot mix thin layer, micro surfacing, fog seal layer and sand fog seal layer. Among them, hot mix thin layer has the highest unit price and consumes a lot of energy, which is not environmentally friendly. Micro surfacing has the disadvantages of high noise and insufficient durability, which has almost become a consensus among road workers. These two are mostly suitable for corrective maintenance operations on roads with slight or moderate diseases. In contrast, in the case of intact pavement structure and slight diseases, if the purpose is to restore or improve the skid resistance of the pavement, the seal pre-curing technology is undoubtedly the most economical and applicable choice.

[0004] The traditional fog seal only sprays a layer of emulsified asphalt or reducing agent, which actually reduces the friction coefficient of the road surface. Although the sand seal technology with improved process adds anti-skid sand to ensure the initial anti-skid ability of the road surface, and can effectively repair small cracks on the road surface and solve the water sealing problem, the comprehensive performance of commercially available emulsified asphalt or modified emulsified asphalt as the binder of the sand seal is relatively weak, resulting in a series of engineering problems such as early peeling and graining of the seal, which restricts the promotion and application of seal maintenance technology. Summary of the invention

[0005] The object of the present invention is to provide an elastic adhesive, a combination product for road sealing, an anti-skid road sealing structure and a preparation method and application thereof. The elastic adhesive provided by the present invention has excellent bonding performance and is resistant to aging.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The invention provides an elastic adhesive. The raw materials of the elastic adhesive include, by weight percentage, 45-55% of petroleum asphalt, 30-40% of water, 0.9-1.2% of acid, 0.8-1.2% of emulsifier, 0.4-1% of stabilizing agent, 3-5% of viscoelastic agent, 2-3% of compatibilizer, 0.5-0.8% of anti-aging agent, 5-6% of polyurethane block copolymer emulsion and 0.2-0.3% of sulfide silane coupling agent.

[0008] Preferably, the petroleum asphalt is Esso 70# asphalt;

[0009] The emulsifier includes alkyl polyamine cationic emulsifier and polyoxyethylene ether nonionic emulsifier;

[0010] The stabilizing agent includes organic agents and inorganic agents;

[0011] The viscoelastic additive includes one or more of linear SBS, linear SEBS and rubber powder;

[0012] The compatibilizer includes palmitoleic acid, aromatic oil or furfural extracted oil;

[0013] The anti-aging agent is 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline;

[0014] The sulfide silane coupling agent is KH-845 reagent.

[0015] The present invention also provides a method for preparing the elastic adhesive described in the above technical solution, comprising the following steps:

[0016] Mixing petroleum asphalt, viscoelastic additive, compatibilizer and anti-aging agent to obtain modified asphalt;

[0017] Mixing an emulsifier, a stabilizing aid, water and an acid to obtain a soap solution;

[0018] mixing the modified asphalt and soap solution to obtain emulsified asphalt;

[0019] The emulsified asphalt, polyurethane block copolymer emulsion and sulfide silane coupling agent are mixed to obtain the elastic adhesive.

[0020] The present invention also provides a combined product for road sealing, comprising an elastic adhesive, anti-skid particles and a reactive sealing agent; the elastic adhesive is the elastic adhesive described in the above technical solution or the elastic adhesive obtained by the preparation method described in the above technical solution;

[0021] The components of the anti-skid particles include 10-15% rubber particles and 85-90% aggregates in terms of mass percentage;

[0022] The raw materials of the reaction cover agent include, by mass percentage, 40-50% petroleum asphalt, 42-52% water, 0.8-1.8% emulsifier, 0.2-0.4% dispersant, 6-10% carboxyl-terminated resin emulsion, 1.2-2% crosslinking agent and 12-15% micron polymer.

[0023] Preferably, the particle size of the rubber particles is 3 to 5 mm;

[0024] The aggregate includes one or more of steel slag, corundum and alkaline aggregate; the alkaline aggregate includes limestone and / or basalt; and the particle size of the aggregate is 1 to 7 mm.

[0025] Preferably, the petroleum asphalt is Esso 70# asphalt;

[0026] The emulsifier is a non-ionic lignin emulsifier;

[0027] The dispersing aid is ammonium chloride;

[0028] The carboxyl-terminated resin emulsion includes alkyd resin, polyester resin, acrylic resin or epoxy resin;

[0029] The cross-linking agent is a methyl etherified hexamethylol melamine cross-linking agent;

[0030] The micron polymer is polypropylene particles.

[0031] Preferably, the method for preparing the reaction cover agent comprises the following steps:

[0032] Mixing an emulsifier, a dispersing aid and water to obtain a soap solution;

[0033] The soap solution and petroleum asphalt are mixed to obtain emulsified asphalt A;

[0034] The emulsified asphalt A is mixed with the carboxyl-terminated resin emulsion to obtain emulsified asphalt B;

[0035] The emulsified asphalt B cross-linking agent and the micron polymer are mixed to obtain the reaction cover agent.

[0036] The present invention also provides an anti-skid road sealing layer structure, comprising an elastic adhesive layer, an anti-skid particle layer and a resin protective layer stacked in sequence; the anti-skid particles in the anti-skid particle layer are embedded with the elastic adhesive layer and the resin protective layer;

[0037] The elastic adhesive layer is made of the elastic adhesive described in the above technical solution or the elastic adhesive obtained by the preparation method described in the above technical solution;

[0038] The anti-skid particle layer is made of the anti-skid particles described in the above technical solution;

[0039] The resin protective layer is prepared from the reaction cover agent described in the above technical solution.

[0040] Preferably, the anti-skid road sealing structure has a thickness of 4.5 to 7.5 mm;

[0041] The thickness of the elastic adhesive layer is 0.6 to 0.8 mm;

[0042] The thickness of the anti-slip granular layer is 3.5 to 6.5 mm;

[0043] The thickness of the resin protective layer is 0.2-0.4 mm.

[0044] The present invention also provides the elastic adhesive described in the above technical solution, the elastic adhesive obtained by the preparation method described in the above technical solution, the combination product described in the above technical solution or the anti-skid road sealing structure described in the above technical solution for use in road maintenance.

[0045] The present invention provides an elastic adhesive, wherein the raw materials of the elastic adhesive include, by mass percentage, 45-55% petroleum asphalt, 30-40% water, 0.9-1.2% acid, 0.8-1.2% emulsifier, 0.4-1% stabilizing agent, 3-5% viscoelastic agent, 2-3% compatibilizer, 0.5-0.8% anti-aging agent, 5-6% polyurethane block copolymer emulsion and 0.2-0.3% sulfide silane coupling agent. The elastic adhesive provided by the present invention is a high-performance emulsified asphalt with fast demulsification, excellent bonding performance and aging resistance, wherein the viscoelastic agent is combined with the polyurethane block copolymer emulsion for composite modification, and after the anti-aging agent is added, the evaporation residue has higher bonding strength and elastic recovery ability than ordinary / modified emulsified asphalt, and better resistance to thermal oxidation aging. Therefore, the elastic adhesive can strongly connect anti-skid particles and improve the comprehensive performance of sand seals.

[0046] In the combined product for road sealing provided by the present invention, the reactive cover agent raw material is cross-linked and cured by a cross-linking agent and a carboxyl-terminated resin emulsion, and the strength of the cured product is formed quickly and the hardness is high. Combined with the viscous effect of the damping particles on the wheels, a resin protective layer with excellent wear resistance, noise reduction and vibration reduction performance and anti-ultraviolet aging performance can be obtained. At the same time, the two high-performance binders of the elastic adhesive and the reactive cover agent in the combined product have a short curing time, fast opening to traffic, and convenient construction, which greatly improves the efficiency of maintenance and construction, reduces the time of opening to traffic, and ensures the long-term service life of the sealing layer.

[0047] The anti-skid road seal structure provided by the present invention adopts a double-layer high-performance adhesive material embedded with damping anti-skid particles. The parts are tightly bonded and have a strong cross-linking effect. It solves the problems of weak performance of the current sand-containing seal adhesive material, poor driving comfort, and short service life. It is more wear-resistant than the traditional sand seal. At the same time, under the synergistic effect of various materials, the anti-skid seal has a significant effect on absorbing tire noise, and the wear loss rate after high temperature or ultraviolet aging is maintained at a low level. It also has both water sealing and anti-skid lifting functions, which has significant engineering significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0049] Figure 1 This is a schematic structural diagram of the anti-skid road sealing structure provided by the present invention, wherein ① is a resin protective layer, ② is an anti-skid granular layer, ③ is an elastic adhesive layer, ④ is a micron polymer in the resin protective layer, and ⑤ is a cement or asphalt pavement to be treated. DETAILED DESCRIPTION

[0050] The invention provides an elastic adhesive. The raw materials of the elastic adhesive include, by weight percentage, 45-55% of petroleum asphalt, 30-40% of water, 0.9-1.2% of acid, 0.8-1.2% of emulsifier, 0.4-1% of stabilizing agent, 3-5% of viscoelastic agent, 2-3% of compatibilizer, 0.5-0.8% of anti-aging agent, 5-6% of polyurethane block copolymer emulsion and 0.2-0.3% of sulfide silane coupling agent.

[0051] In the present invention, unless otherwise specified, all raw material components are commercially available products well known to those skilled in the art.

[0052] In terms of mass percentage, the raw material of the elastic adhesive of the present invention includes 45-55% petroleum asphalt, preferably 47-53%; the petroleum asphalt is preferably Esso 70# asphalt.

[0053] Calculated by mass percentage, the raw materials of the elastic adhesive of the present invention include 30-40% water, preferably 32-38%.

[0054] In terms of mass percentage, the raw materials of the elastic adhesive of the present invention include 0.9-1.2% acid, preferably 1-1.1%; the acid is preferably hydrochloric acid or phosphoric acid, more preferably hydrochloric acid; the concentration of the hydrochloric acid is preferably 25-36%, more preferably 30-36%.

[0055] In terms of mass percentage, the raw materials of the elastic adhesive of the present invention include 0.8-1.2% of emulsifier, preferably 0.9-1.1%; the emulsifier preferably includes an alkyl polyamine cationic emulsifier and a polyoxyethylene ether nonionic emulsifier; the alkyl polyamine cationic emulsifier is preferably a Weiswick model RE-611 alkyl polyamine cationic emulsifier; the polyoxyethylene ether nonionic emulsifier is preferably a Tianjin Hongyang Chemical model OP-30 polyoxyethylene ether nonionic emulsifier; the mass ratio of the alkyl polyamine cationic emulsifier to the polyoxyethylene ether nonionic emulsifier is preferably 1-3:1, more preferably 2-3:1.

[0056] In the present invention, the emulsifier can match the HLB values ​​of different modified asphalts after compounding and has more hydrophilic groups, which can improve the emulsification ability and adjust the demulsification speed and storage stability of the emulsified asphalt.

[0057] In terms of mass percentage, the raw materials of the elastic adhesive of the present invention include 0.4-1% of a stabilizing agent, preferably 0.6-0.8%; the stabilizing agent preferably includes an organic agent and an inorganic agent; the organic agent preferably includes polyacrylamide, polyethylene glycol or hydrocarbon ethyl cellulose, more preferably polyacrylamide or polyethylene glycol; the inorganic agent preferably includes calcium chloride, sodium silicate or sodium phosphate, more preferably calcium chloride or sodium silicate; the mass ratio of the organic agent to the inorganic agent is preferably 1-5:1, more preferably 1-3:1.

[0058] In terms of mass percentage, the raw materials of the elastic adhesive of the present invention include 3-5%, preferably 4-5% of viscoelastic additive; the viscoelastic additive preferably includes one or more of linear SBS, linear SEBS and rubber powder, more preferably linear SBS and / or linear SEBS.

[0059] In the present invention, the viscoelastic additive can improve the performance indicators such as softening point, ductility, dynamic viscosity and elastic recovery of the emulsified asphalt evaporation residue after being added.

[0060] In terms of mass percentage, the raw materials of the elastic adhesive of the present invention include 2-3% of a compatibilizer, preferably 2.2-2.8%; the compatibilizer preferably includes palmitoleic acid, aromatic oil or furfural extracted oil, more preferably palmitoleic acid or aromatic oil.

[0061] In terms of mass percentage, the raw materials of the elastic adhesive of the present invention include 0.5-0.8%, preferably 0.6-0.7% of an anti-aging agent; the anti-aging agent is preferably 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline.

[0062] In the present invention, the 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline is a light brown viscous liquid, which can improve the thermal oxidation aging resistance of asphalt.

[0063] In terms of mass percentage, the raw materials of the elastic adhesive of the present invention include 5-6% polyurethane block copolymer emulsion, preferably 5.5-6%; the solid content of the polyurethane block copolymer emulsion is preferably 35-40%, more preferably 40%.

[0064] In the present invention, the polyurethane block copolymer emulsion can improve the toughness and fatigue resistance of the emulsified asphalt evaporation residue.

[0065] In terms of mass percentage, the raw materials of the elastic adhesive of the present invention include 0.2-0.3% of sulfide silane coupling agent, preferably 0.25-0.3%; the sulfide silane coupling agent is preferably KH-845 reagent; the mass percentage of the effective ingredient in the KH-845 reagent is preferably >98%, and the density is preferably 1.089±0.005g / cm 3 .

[0066] In the present invention, the KH-845 reagent is a light yellow transparent liquid, which can maintain the vulcanization balance of the emulsion system and enhance the cross-linking effect.

[0067] The elastic adhesive provided by the present invention is a high-performance emulsified asphalt with fast demulsification, excellent bonding performance and aging resistance. It adopts elastic polymer modifier combined with polyurethane block copolymer emulsion for composite modification. After adding anti-aging agent, its evaporation residue has higher bonding strength and elastic recovery ability than ordinary / modified emulsified asphalt, and better resistance to thermal oxidation aging. Therefore, the elastic adhesive can strongly connect anti-skid particles and improve the comprehensive performance of sand seal. In addition, the elastic adhesive adopts emulsifier compound to increase active groups to enhance emulsification ability, and preferably stabilizes the combination of auxiliary agents to improve storage stability. Compared with ordinary / modified emulsified asphalt, it has faster demulsification during spraying construction.

[0068] The present invention also provides a method for preparing the elastic adhesive described in the above technical solution, comprising the following steps:

[0069] Mixing petroleum asphalt, viscoelastic additive, compatibilizer and anti-aging agent to obtain modified asphalt;

[0070] Mixing an emulsifier, a stabilizing aid, water and an acid to obtain a soap solution;

[0071] mixing the modified asphalt and soap solution to obtain emulsified asphalt;

[0072] The emulsified asphalt, polyurethane block copolymer emulsion and sulfide silane coupling agent are mixed to obtain the elastic adhesive.

[0073] The invention mixes petroleum asphalt, a viscoelastic additive, a compatibilizer and an anti-aging agent to obtain modified asphalt.

[0074] In the present invention, the mixing process is preferably: first heating and melting the petroleum asphalt, then raising the temperature, adding a viscoelastic additive, a compatibilizer and an anti-aging agent and then stirring; the heating and melting temperature is preferably 135-140°C; the heating time is preferably 10-15min, and the target temperature is preferably 180-185°C; the stirring speed is preferably 2000-3500rpm, more preferably 2500-3000rpm; the time is preferably 1.5-2.5h, more preferably 2-2.5h; the stirring equipment is preferably a multi-layer propulsion stirring blade; the stirring is preferably further preferably including growth; the growth time is preferably 1-2h.

[0075] The present invention mixes an emulsifier, a stabilizing auxiliary agent, water and an acid to obtain a soap solution.

[0076] The present invention has no special limitation on the mixing process, and a method well known to those skilled in the art may be adopted; in the present invention, the pH of the soap solution is preferably 2 to 2.5.

[0077] After obtaining the modified asphalt and the soap solution, the present invention mixes the modified asphalt and the soap solution to obtain emulsified asphalt.

[0078] In the present invention, the temperature of the modified asphalt is preferably 180-185°C; the temperature of the soap solution is preferably 60-70°C; the mixing speed is preferably 3000-3500 rpm, and the time is preferably 2-3 min; the mixing equipment is preferably a high shear colloid mill.

[0079] After obtaining the emulsified asphalt, the present invention mixes the emulsified asphalt, polyurethane block copolymer emulsion and sulfide silane coupling agent to obtain the elastic adhesive.

[0080] In the present invention, the mixing speed is preferably 1000-1500 rpm, and the mixing time is preferably 30-45 min; the elastic adhesive is preferably stored in a cool and sealed place.

[0081] The present invention also provides a combined product for road sealing, comprising an elastic adhesive, anti-skid particles and a reactive sealing agent; the elastic adhesive is the elastic adhesive described in the above technical solution or the elastic adhesive obtained by the preparation method described in the above technical solution;

[0082] The components of the anti-skid particles include 10-15% rubber particles and 85-90% aggregates in terms of mass percentage;

[0083] The raw materials of the reaction cover agent include, by mass percentage, 40-50% petroleum asphalt, 42-52% water, 0.8-1.8% emulsifier, 0.2-0.4% dispersant, 6-10% carboxyl-terminated resin emulsion, 1.2-2% crosslinking agent and 12-15% micron polymer.

[0084] In terms of mass percentage, the anti-skid particles of the present invention include 10-15% of rubber particles, preferably 11-14%; the particle size of the rubber particles is preferably 3-5 mm, more preferably 4-5 mm.

[0085] In terms of mass percentage, the components of the anti-skid particles of the present invention include 85-90% aggregate, preferably 86-89%; the aggregate preferably includes one or more of steel slag, corundum and alkaline aggregate, more preferably corundum and / or alkaline aggregate; the alkaline aggregate preferably includes limestone and / or basalt, more preferably basalt; the particle size of the aggregate is preferably 1-7 mm, more preferably 1-5 mm.

[0086] When the thickness of the anti-skid road seal structure is 4.5-5.5 mm, the components of the anti-skid particles are preferably 10-15% of 3-5 mm rubber particles, 42-52% of 1-3 mm aggregates and 35-45% of 3-5 mm aggregates, more preferably 11-14% of 3-5 mm rubber particles, 45-50% of 1-3 mm aggregates and 38-42% of 3-5 mm aggregates.

[0087] When the thickness of the anti-skid road seal structure is 5.5-6.5 mm, the components of the anti-skid particles are preferably 10-15% of 3-5 mm rubber particles, 5-10% of 1-3 mm aggregates, 60-70% of 3-5 mm aggregates and 10-20% of 5-7 mm aggregates, more preferably 11-14% of 3-5 mm rubber particles, 6-8% of 1-3 mm aggregates, 62-68% of 3-5 mm aggregates and 12-18% of 5-7 mm aggregates.

[0088] When the thickness of the anti-skid road seal structure is 6.5-7.5 mm, the components of the anti-skid particles are preferably 10-15% of 3-5 mm rubber particles, 25-35% of 1-3 mm aggregates, 20-24% of 3-5 mm aggregates and 30-40% of 5-7 mm aggregates, more preferably 11-14% of 3-5 mm rubber particles, 28-32% of 1-3 mm aggregates, 21-23% of 3-5 mm aggregates and 32-38% of 5-7 mm aggregates.

[0089] In the present invention, the high anti-skid performance of the seal layer is maintained by reasonably designing the type, gradation and thickness of anti-skid particles, and the viscosity and comprehensive damping effect of elastic adhesives, rubber particles and micron polymers are combined. Compared with the single-particle sand seal layer, the driving safety of the seal layer is guaranteed and better driving comfort is provided.

[0090] Calculated by mass percentage, the raw materials of the reactive cover agent of the present invention include 40-50% petroleum asphalt, preferably 40-45%; the petroleum asphalt is preferably Esso 70# asphalt.

[0091] Calculated by mass percentage, the raw materials of the reaction cover agent of the present invention include 42-52% water, preferably 45-50%.

[0092] Calculated by mass percentage, the raw materials of the reaction cover agent of the present invention include 0.8-1.8% of emulsifier, preferably 1-1.5%; the emulsifier is preferably a non-ionic lignin emulsifier.

[0093] In terms of mass percentage, the raw materials of the reaction cover agent of the present invention include 0.2-0.4% of a dispersing aid, preferably 0.3-0.4%; the dispersing aid is preferably ammonium chloride.

[0094] In terms of mass percentage, the raw materials of the reactive cover agent of the present invention include 6-10% of terminal carboxyl resin emulsion, preferably 7-9%; the solid content of the terminal carboxyl resin emulsion is preferably 45-55%, more preferably 50-55%; the terminal carboxyl resin emulsion preferably includes alkyd resin, polyester resin, acrylic resin or epoxy resin, more preferably polyester resin, acrylic resin or epoxy resin; the epoxy resin is preferably E-51 water-based epoxy resin emulsion.

[0095] In terms of mass percentage, the raw materials of the reactive cover agent of the present invention include 1.2-2%, preferably 1.4-1.8% of a crosslinking agent; the crosslinking agent is preferably a methyl etherified hexahydroxymethyl melamine crosslinking agent.

[0096] In terms of mass percentage, the raw materials of the reaction cover agent of the present invention include 12-15% of micron polymer, preferably 13-15%; the micron polymer is preferably polypropylene particles; the particle size of the polypropylene particles is preferably 60-80 mesh; the molecular weight of the polypropylene particles is preferably 120,000-150,000.

[0097] Preferably, the method for preparing the reaction cover agent comprises the following steps:

[0098] Mixing an emulsifier, a dispersing aid and water to obtain a soap solution;

[0099] The soap solution and petroleum asphalt are mixed to obtain emulsified asphalt A;

[0100] The emulsified asphalt A is mixed with the carboxyl-terminated resin emulsion to obtain emulsified asphalt B;

[0101] The emulsified asphalt B cross-linking agent and the micron polymer are mixed to obtain the reaction cover agent.

[0102] The present invention mixes an emulsifier, a dispersing aid and water to obtain a soap solution.

[0103] In the present invention, the mixing device is preferably a high shear colloid mill; the mixing temperature is preferably 50-55°C, and the mixing time is preferably 1-2 minutes; and the insulation temperature of the soap solution is preferably 50-55°C.

[0104] After obtaining the soap solution, the present invention mixes the soap solution with petroleum asphalt to obtain emulsified asphalt A.

[0105] In the present invention, the mixing process preferably further includes heating and melting the petroleum asphalt before mixing; the heating and melting temperature is preferably 135-140°C; the mixing equipment is preferably a high shear colloid mill; the mixing speed is preferably 3000-3500rpm, and the mixing time is preferably 5-10min.

[0106] After obtaining the emulsified asphalt A, the present invention mixes the emulsified asphalt A with a carboxyl-terminated resin emulsion to obtain emulsified asphalt B.

[0107] In the present invention, the mixing device is preferably an electric stirrer; the mixing speed is preferably 400-500 rpm, and the temperature is preferably room temperature; the present invention does not have any special limitation on the mixing time, and the mixing can be carried out until uniform.

[0108] After obtaining the emulsified asphalt B, the present invention mixes the emulsified asphalt B cross-linking agent and the micron polymer to obtain the reaction capping agent.

[0109] In the present invention, the mixing speed is preferably 200-300 rpm, and the temperature is preferably room temperature; the present invention does not have any special limitation on the mixing time, and the mixing can be carried out until uniform.

[0110] In the combined product for road sealing provided by the present invention, the reactive cover agent raw material is cross-linked and cured by a cross-linking agent and a carboxyl-terminated resin emulsion, and the strength of the cured product is formed quickly and the hardness is high. Combined with the viscous effect of the damping particles on the wheels, a resin protective layer with excellent wear resistance, noise reduction and vibration reduction performance and anti-ultraviolet aging performance can be obtained. At the same time, the two high-performance binders of the elastic adhesive and the reactive cover agent in the combined product have a short curing time, fast opening to traffic, and convenient construction, which greatly improves the efficiency of maintenance and construction, reduces the time of opening to traffic, and ensures the long-term service life of the sealing layer.

[0111] The present invention also provides an anti-skid road sealing layer structure, comprising an elastic adhesive layer, an anti-skid particle layer and a resin protective layer stacked in sequence; the anti-skid particles in the anti-skid particle layer are embedded with the elastic adhesive layer and the resin protective layer;

[0112] The elastic adhesive layer is made of the elastic adhesive described in the above technical solution or the elastic adhesive obtained by the preparation method described in the above technical solution;

[0113] The anti-skid particle layer is made of the anti-skid particles described in the above technical solution;

[0114] The resin protective layer is prepared from the reaction cover agent described in the above technical solution.

[0115] In the present invention, the thickness of the anti-skid road sealing structure is preferably 4.5 to 7.5 mm, more preferably 5 to 7 mm.

[0116] In the present invention, the thickness of the elastic adhesive layer is preferably 0.6 to 0.8 mm, more preferably 0.7 to 0.8 mm.

[0117] In the present invention, the thickness of the anti-slip granular layer is preferably 3.5 to 6.5 mm, more preferably 4 to 6 mm.

[0118] In the present invention, the thickness of the resin protective layer is preferably 0.2 to 0.4 mm, more preferably 0.3 to 0.4 mm.

[0119] In the present invention, the method for preparing the anti-skid road sealing structure preferably comprises the following steps:

[0120] Spreading the elastic adhesive to obtain an elastic adhesive layer;

[0121] Spreading anti-skid particles on the surface of the elastic adhesive layer to obtain an anti-skid particle layer;

[0122] The reaction sealing agent is spread on the surface of the anti-skid particle layer to obtain a resin protective layer, that is, the anti-skid road sealing layer structure is obtained.

[0123] The present invention spreads the elastic adhesive to obtain the elastic adhesive layer.

[0124] In the present invention, the elastic adhesive spraying amount is preferably 0.8 to 1.3 kg / m 2 , more preferably 0.9 to 1.2 kg / m 2 .

[0125] After obtaining the elastic adhesive layer, the present invention sprinkles anti-skid particles on the surface of the elastic adhesive layer to obtain an anti-skid particle layer.

[0126] In the present invention, the components of the anti-skid particles include 10-15% rubber particles and 85-90% aggregates in terms of mass percentage; the rubber particles and aggregates are preferably dusted and mixed in sequence before being spread; the dusting and mixing equipment is preferably a mixing plant.

[0127] In the present invention, the spraying amount of the anti-skid particles is preferably 4.5 to 6 kg / m 2 , more preferably 5 to 5.5 kg / m 2 ; The elastic adhesive and anti-skid particles are preferably spread synchronously by a synchronous sealing vehicle; The elastic adhesive and anti-skid particles are preferably spread synchronously.

[0128] In the present invention, after obtaining the anti-skid granular layer, rolling is preferably further included; the rolling equipment is preferably a roller; the roller is preferably a 3-5 t double-rubber wheel roller; the number of rolling is preferably 1-2 times.

[0129] In the present invention, the elastic adhesive layer and the anti-slip particle layer form a highly elastic and wear-resistant bottom layer, and the highly elastic and wear-resistant bottom layer forms a final strength after waiting for about 1 hour.

[0130] After obtaining the anti-skid particle layer, the present invention sprinkles a reactive sealing agent on the surface of the anti-skid particle layer to obtain a resin protective layer, that is, to obtain the anti-skid road sealing layer structure.

[0131] In the present invention, the spraying amount of the reaction cover agent is preferably 0.3 to 0.6 kg / m 2 , more preferably 0.4 to 0.5 kg / m 2 ; The spraying equipment for the reaction cover agent is preferably a special spraying vehicle for the reaction cover agent; and the spraying is preferably pressurized spraying.

[0132] In the present invention, after obtaining the resin protective layer, curing is preferably further performed; the curing time is preferably 1 to 2 hours.

[0133] In the present invention, an anti-skid sealing layer with damping effect and anti-aging can be formed after curing is completed. After secondary rolling by subsequent wheels, the gripping state of the anti-skid particles gradually stabilizes and the surface of the sealing layer tends to be flat.

[0134] The anti-skid road seal structure provided by the present invention adopts a double-layer high-performance adhesive material embedded with damping anti-skid particles. The parts are tightly bonded and have a strong cross-linking effect. It solves the problems of weak performance of the current sand-containing seal adhesive material, poor driving comfort, and short service life. It is more wear-resistant than the traditional sand seal. At the same time, under the synergistic effect of various materials, the anti-skid seal has a significant effect on absorbing tire noise, and the wear loss rate after high temperature or ultraviolet aging is maintained at a low level. It also has both water sealing and anti-skid lifting functions, which has significant engineering significance.

[0135] The technical advantages of the method for preparing anti-skid road sealing materials provided by the present invention are: (1) the material preparation process is relatively simple, the construction can be carried out at room temperature, and the overall process is safe and simple; (2) the composition structure of the sealing material is optimized, the maintenance time is shortened to the maximum extent, the daily work efficiency is significantly improved, the anti-aging and noise reduction functions are added, and the service life of the sealing layer is effectively improved; (3) compared with the one-oil-one-sand or pure emulsion spreading process, the double-layer binder embedded structure and multiple rolling ensure the bonding effect of the anti-skid particles.

[0136] The present invention also provides the elastic adhesive described in the above technical solution, the elastic adhesive obtained by the preparation method described in the above technical solution, the combination product described in the above technical solution or the anti-skid road sealing structure described in the above technical solution for use in road maintenance.

[0137] The present invention does not have any special limitation on the application process of the elastic adhesive, the combination product or the anti-skid road sealing structure in road maintenance, and any method familiar to those skilled in the art may be used.

[0138] In order to further illustrate the present invention, the elastic adhesive, the combination product for road sealing, the anti-skid road sealing structure and the preparation method and application thereof provided by the present invention are described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0139] The structural schematic diagram of the anti-skid road sealing structure provided by the present invention is shown in Figure 1 , where ① is the resin protective layer, ②

[0140] The first is the anti-skid particle layer, the second is the elastic adhesive layer, the third is the micron polymer in the resin protective layer, and the fourth is the cement or asphalt pavement to be treated.

[0141] Example 1

[0142] According to the mass fraction, 50% 70# Esso asphalt was heated to 135°C for melting, and then heated to 180°C at a heating rate of 5°C / min within 15 minutes. 4% SBS, 2% aromatic oil, 0.6% 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline and the above asphalt were mixed, and stirred at 3500r / min for 2 hours using a multi-layer propulsion stirring blade, and then grown for 1.5 hours to obtain a modified asphalt. 0.6% alkyl polyamine cationic emulsifier, 0.2% OP-30 polyoxyethylene ether nonionic emulsion, 0.2% Polyethylene glycol, 0.2% calcium chloride and 35% water are mixed, and 1% hydrochloric acid is added to adjust the pH value to 2-2.5 to obtain soap solution; the modified asphalt is heated to 180°C and placed in the asphalt tank of a high shear colloid mill, and the 60°C soap solution is added, and emulsified at 3000r / min for 3min to obtain modified emulsified asphalt; 6% polyurethane block copolymer emulsion, 0.2% KH-845 sulfide silane coupling agent and modified emulsified asphalt are stirred at 1500r / min for 30min, and then stored in a cool and sealed place to obtain an elastic adhesive.

[0143] According to the mass fraction, 1.1% non-ionic lignin emulsifier, 0.3% ammonium chloride and 49% water are mixed evenly, kept warm at 50°C, placed in a high shear colloid mill for circulation for 2 minutes to obtain a soap solution; 40% 70# Esso asphalt is heated to 135°C, placed in a colloid mill in a flowing state, and circulated and sheared for 5 minutes at 3500r / min to obtain a first emulsified asphalt; the first emulsified asphalt and 8% end carboxyl resin emulsion are stirred evenly at room temperature with an electric stirrer at a stirring speed of 500r / min to obtain a second emulsified asphalt; the second emulsified asphalt and 1.6% methyl etherified hexahydroxymethyl melamine cross-linking agent and 15% externally added micron suspended matter are stirred evenly at room temperature at a stirring speed of 300r / min to obtain a reaction cover agent.

[0144] Table 1 Composition of anti-skid particles in Example 1

[0145]

[0146] Use a synchronous sealing vehicle to simultaneously spread the elastic adhesive and anti-skid particles onto the original road surface to be treated to form a highly elastic and wear-resistant bottom layer. The amount of elastic adhesive spread is 1.2 kg / m 2 The spreading amount of anti-skid particles is 5.5kg / m 2 , forming a high-elastic wear-resistant bottom layer with preliminary strength, and then using a 3t double-rubber wheel roller to roll it twice, waiting for 1 hour, to obtain a high-elastic wear-resistant bottom layer with final strength;

[0147] Use a special spraying vehicle for reactive cover agent to spray the reactive cover agent at a rate of 0.3kg / m 2The high-elastic wear-resistant base layer is sprayed under pressure, cured for 1 hour, and rolled for the second time to form a surface resin protective layer on the surface of the high-elastic wear-resistant base layer to obtain an anti-skid road seal layer.

[0148] Example 2

[0149] According to the mass fraction, 45% 70# Esso asphalt was heated to 135°C for melting, and then heated to 180°C at a heating rate of 5°C / min within 15 minutes. 4% SBS, 3% aromatic oil, 0.8% 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline and the above asphalt were mixed, and stirred at 3500r / min for 2 hours using a multi-layer propulsion stirring blade, and then grown for 1 hour to obtain a modified asphalt. 0.9% alkyl polyamine cationic emulsifier, 0.3% OP-30 polyoxyethylene ether non-ionic emulsion, 0.3% polyethylene glycol were added. Alcohol, 0.3% calcium chloride and 38.2% water are mixed, and 0.9% hydrochloric acid is added to adjust the pH value to 2-2.5 to obtain soap solution; the modified asphalt is heated to 180°C and placed in the asphalt tank of a high shear colloid mill, and the 60°C soap solution is added, and emulsified at 3500r / min for 3min to obtain modified emulsified asphalt; 6% polyurethane block copolymer emulsion, 0.3% KH-845 sulfide silane coupling agent and modified emulsified asphalt are stirred at 1500r / min for 30min, and then stored in a cool and sealed place to obtain an elastic adhesive.

[0150] According to the mass fraction, 1.5% non-ionic lignin emulsifier, 0.3% ammonium chloride and 46% water are mixed evenly, kept warm at 50°C, placed in a high shear colloid mill for circulation for 2 minutes to obtain a soap solution; 45% 70# Esso asphalt is heated to 135°C, placed in a colloid mill in a flowing state, and circulated and sheared for 5 minutes at 3500r / min to obtain a first emulsified asphalt; the first emulsified asphalt and 6% terminal carboxyl resin emulsion are stirred evenly at room temperature with an electric stirrer at a stirring speed of 500r / min to obtain a second emulsified asphalt; the second emulsified asphalt and 1.2% methyl etherified hexahydroxymethyl melamine cross-linking agent and 15% externally added micron suspended matter are stirred evenly at room temperature at a stirring speed of 300r / min to obtain a reaction cover agent.

[0151] Table 2 Composition of anti-skid particles in Example 2

[0152]

[0153] Use a synchronous sealing vehicle to simultaneously spread the elastic adhesive and anti-skid particles onto the original road surface to be treated to form a highly elastic and wear-resistant bottom layer. The amount of elastic adhesive spread is 1.2 kg / m 2 The spreading amount of anti-skid particles is 5.5kg / m 2, forming a high-elastic wear-resistant bottom layer with preliminary strength, and then using a 3t double-rubber wheel roller to roll it twice, waiting for 1 hour, to obtain a high-elastic wear-resistant bottom layer with final strength;

[0154] Use a special spraying vehicle for reactive cover agent to spray the reactive cover agent at a rate of 0.3kg / m 2 The high-elastic wear-resistant base layer is sprayed under pressure, cured for 1 hour, and rolled for the second time to form a surface resin protective layer on the surface of the high-elastic wear-resistant base layer to obtain an anti-skid road seal layer.

[0155] Example 3

[0156] According to the mass fraction, 53% 70# Esso asphalt was heated to 135°C for melting, and then heated to 180°C at a heating rate of 5°C / min within 10 minutes. 4% SBS, 2% aromatic oil, 0.5% 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline and the above asphalt were mixed, and stirred at 3500r / min for 2 hours using a multi-layer propulsion stirring blade, and then grown for 1 hour to obtain a modified asphalt. 0.9% alkyl polyamine cationic emulsifier, 0.3% OP-30 polyoxyethylene ether nonionic emulsion, 0.4% polyethylene Diol, 0.4% calcium chloride and 31% water are mixed, and 1.2% hydrochloric acid is added to adjust the pH value to 2-2.5 to obtain soap solution; the modified asphalt is heated to 180°C and placed in the asphalt tank of a high shear colloid mill, and the 60°C soap solution is added, and emulsified at 3500r / min for 3min to obtain modified emulsified asphalt; 6% polyurethane block copolymer emulsion, 0.3% KH-845 sulfide silane coupling agent and modified emulsified asphalt are stirred at 1500r / min for 30min, and then stored in a cool and sealed place to obtain an elastic adhesive.

[0157] According to the mass fraction, 1% non-ionic lignin emulsifier, 0.3% ammonium chloride and 42% water are mixed evenly, kept warm at 50°C, placed in a high shear colloid mill for circulation for 2 minutes to obtain a soap solution; 44.7% 70# Esso asphalt is heated to 135°C, placed in a colloid mill in a flowing state, and circulated and sheared for 5 minutes at 3000r / min to obtain a first emulsified asphalt; the first emulsified asphalt and 10% terminal carboxyl resin emulsion are stirred evenly at room temperature with an electric stirrer at a stirring speed of 500r / min to obtain a second emulsified asphalt; the second emulsified asphalt and 2% methyl etherified hexahydroxymethyl melamine cross-linking agent and 15% externally added micron suspended matter are stirred evenly at room temperature at a stirring speed of 300r / min to obtain a reaction cover agent.

[0158] Table 3 Composition of anti-skid particles in Example 3

[0159]

[0160] Use a synchronous sealing vehicle to simultaneously spread the elastic adhesive and anti-skid particles onto the original road surface to be treated to form a highly elastic and wear-resistant bottom layer. The amount of elastic adhesive spread is 1.2 kg / m 2 The spreading amount of anti-skid particles is 5.5kg / m 2 , forming a high-elastic wear-resistant bottom layer with preliminary strength, and then using a 3t double-rubber wheel roller to roll it twice, waiting for 1 hour, to obtain a high-elastic wear-resistant bottom layer with final strength;

[0161] Use a special spraying vehicle for reactive cover agent to spray the reactive cover agent at a rate of 0.3kg / m 2 The high-elastic wear-resistant base layer is sprayed under pressure, cured for 1 hour, and rolled for the second time to form a surface resin protective layer on the surface of the high-elastic wear-resistant base layer to obtain an anti-skid road seal layer.

[0162] Test Example 1

[0163] The performance of the elastic adhesive described in Example 1 and common emulsified asphalt and modified emulsified asphalt on the market were tested, and the results are shown in Table 4.

[0164] Table 4 Comparison of the effects of the elastic adhesive, common emulsified asphalt and modified emulsified asphalt described in Example 1

[0165]

[0166]

[0167] It can be seen from the results in Table 4 that the various indicators of the elastic adhesive in the present invention are significantly superior to those of ordinary emulsified asphalt and modified emulsified asphalt: high solid content, fast demulsification speed, and the bonding performance with the interface is more than doubled; from the three major indicators of asphalt residue and elastic recovery rate, the elastic adhesive has excellent high and low temperature performance and elastic recovery ability; at the same time, the elastic adhesive has a higher damping factor and also has better noise reduction potential.

[0168] Test Example 2

[0169] The performance of the anti-slip seal layers described in Examples 1 to 3 was tested, and the test results are shown in Table 5.

[0170] Table 5 Performance test results of the anti-slip seal layer described in Examples 1 to 3

[0171] Technical indicators Example 1 Example 2 Example 3 IRI flatness (m / km) 1.14 1.34 1.97 25℃ tensile strength (cement pavement, MPa) 0.41 0.47 0.35 25℃ pull-out strength (asphalt pavement, MPa) 0.28 0.45 0.36 Accelerated loading particle loss rate after high temperature aging test (%) 3.2 1.8 1.9 Particle loss rate of four-wheel abrasion test after UV aging (%) 2.1 0.7 2.4 SFC average 58 63 61 <![CDATA[Permeability coefficient (ml·min -1 )]]> 0 0 0 Tire noise reduction (dB) 3.3 4.1 3.7

[0172] It can be seen from the results in Table 5 that, compared with Examples 1 to 3, under the synergistic enhancement of the viscoelastic additive, the polyurethane block copolymer emulsion and the KH-845 sulfide silane coupling agent, the overall bonding performance of the anti-skid seal layer is significantly improved, and the risk of peeling and falling particles is reduced; the gradation design of adding rubber particles and the buffering effect of the elastic binder can not only ensure the excellent anti-skid performance of the seal layer, but also have a greater effect on weakening tire noise; the anti-aging properties of 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline and the stability of the cross-linking reaction product of the terminal carboxyl resin emulsion and methylated hexahydroxymethylmelamine provide the seal layer with excellent weather resistance.

[0173] It can be seen from the above embodiments that in the anti-skid road seal layer prepared by the present invention, the elastic adhesive material has strong interlayer bonding with the original (cement / asphalt) pavement and the anti-skid particles, and has excellent water-tightness; after the anti-skid particles are graded, the surface macrostructure is large, flat and wear-resistant, which can reduce noise and vibration while improving the anti-skid performance, thereby improving driving comfort; the wear mass loss rate of the anti-skid seal layer after high temperature or ultraviolet aging is at a relatively low level, the comprehensive anti-aging performance is excellent, the various parts are tightly bonded, and the durability is excellent.

[0174] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. An elastic adhesive, characterized in that: The raw materials of the elastic adhesive include, by mass percentage, 45-55% petroleum asphalt, 30-40% water, 0.9-1.2% acid, 0.8-1.2% emulsifier, 0.4-1% stabilizing agent, 3-5% viscoelastic agent, 2-3% compatibilizer, 0.5-0.8% anti-aging agent, 5-6% polyurethane block copolymer emulsion and 0.2-0.3% sulfide silane coupling agent.

2. The elastic adhesive according to claim 1, characterized in that The petroleum asphalt is Esso 70# asphalt; The emulsifier includes alkyl polyamine cationic emulsifier and polyoxyethylene ether nonionic emulsifier; The stabilizing agent includes organic agents and inorganic agents; The viscoelastic additive includes one or more of linear SBS, linear SEBS and rubber powder; The compatibilizer includes palmitoleic acid, aromatic oil or furfural extracted oil; The anti-aging agent is 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline; The sulfide silane coupling agent is KH-845 reagent.

3. The method for preparing the elastic adhesive according to claim 1 or 2, characterized in that: The following steps are involved: Mixing petroleum asphalt, viscoelastic additive, compatibilizer and anti-aging agent to obtain modified asphalt; Mixing an emulsifier, a stabilizing aid, water and an acid to obtain a soap solution; mixing the modified asphalt and soap solution to obtain emulsified asphalt; The emulsified asphalt, polyurethane block copolymer emulsion and sulfide silane coupling agent are mixed to obtain the elastic adhesive.

4. A combination product for road sealing, characterized in that: It comprises an elastic adhesive, anti-slip particles and a reactive cover agent; the elastic adhesive is the elastic adhesive according to claim 1 or 2 or the elastic adhesive obtained by the preparation method according to claim 3; The components of the anti-skid particles include 10-15% rubber particles and 85-90% aggregates in terms of mass percentage; The raw materials of the reaction cover agent include, by mass percentage, 40-50% petroleum asphalt, 42-52% water, 0.8-1.8% emulsifier, 0.2-0.4% dispersant, 6-10% carboxyl-terminated resin emulsion, 1.2-2% crosslinking agent and 12-15% micron polymer.

5. The combination product according to claim 4, characterized in that The particle size of the rubber particles is 3 to 5 mm; The aggregate includes one or more of steel slag, corundum and alkaline aggregate; the alkaline aggregate includes limestone and / or basalt; and the particle size of the aggregate is 1 to 7 mm.

6. The combination product according to claim 4, characterized in that: The petroleum asphalt is Esso 70# asphalt; The emulsifier is a non-ionic lignin emulsifier; The dispersing aid is ammonium chloride; The carboxyl-terminated resin emulsion includes alkyd resin, polyester resin, acrylic resin or epoxy resin; The cross-linking agent is a methyl etherified hexamethylol melamine cross-linking agent; The micron polymer is polypropylene particles.

7. The combination product according to claim 4, characterized in that The preparation method of the reaction cover agent comprises the following steps: Mixing an emulsifier, a dispersing aid and water to obtain a soap solution; The soap solution and petroleum asphalt are mixed to obtain emulsified asphalt A; The emulsified asphalt A is mixed with the carboxyl-terminated resin emulsion to obtain emulsified asphalt B; The emulsified asphalt B cross-linking agent and the micron polymer are mixed to obtain the reaction cover agent.

8. An anti-skid road sealing structure, characterized in that: It comprises an elastic adhesive layer, an anti-skid particle layer and a resin protective layer which are stacked in sequence; the anti-skid particles in the anti-skid particle layer are embedded with the elastic adhesive layer and the resin protective layer; The elastic adhesive layer is made of the elastic adhesive according to claim 1 or 2 or the elastic adhesive obtained by the preparation method according to claim 3; The anti-skid particle layer is made of the anti-skid particles according to claim 4 or 5; The resin protective layer is made from the reactive cover agent described in claim 4, 6 or 7.

9. The anti-skid road sealing structure according to claim 8, characterized in that: The thickness of the anti-skid road sealing structure is 4.5 to 7.5 mm; The thickness of the elastic adhesive layer is 0.6 to 0.8 mm; The thickness of the anti-slip granular layer is 3.5 to 6.5 mm; The thickness of the resin protective layer is 0.2-0.4 mm.

10. Use of the elastic adhesive according to claim 1 or 2, the elastic adhesive obtained by the preparation method according to claim 3, the combination product according to claims 4 to 7 or the anti-skid road sealing structure according to claim 8 or 9 in road maintenance.