Magnetic abrasive and preparation method thereof
Through the embedding method, the gradient hard diffusion seepage layer is formed on the magnetic abrasive, which solves the problems of insufficient life and poor self-sharpness of the magnetic abrasive, and realizes efficient and long-life magnetic abrasives, which improves the processing efficiency and surface light of magnetic abrasives. Overall quality.
Patent Information
- Application Number
- CN202411130224.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
The existing magnetic abrasives have insufficient life, low spherical shape and poor self-sharpness, resulting in low magnetic grinding processing efficiency and poor surface finishing quality.
The magnetic abrasive is prepared by the embedding and seepage method, forming a gradient-distributed hard diffusion permeability layer on the surface of the ferromagnetic phase matrix to form a multi-layer core-shell structure to improve the spherical shape and self-sharpness of the abrasive.
It extends the service life of magnetic abrasives, improves grinding efficiency and surface light finishing quality, and realizes a high-performance magnetic abrasive with simple process and low cost.
Smart Images

Figure CN119019983A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of new materials, and in particular to a magnetic abrasive and a preparation method thereof. Background Art
[0002] Magnetic abrasive finishing (MAF) is a new and efficient surface processing technology. Compared with traditional mechanical processing methods (grinding, belt polishing, etc.), it has the advantages of high processing quality, wide application range, flexible processing, good self-sharpening, and easy automation. It can effectively remove scratches, burrs, curling and other defects on the surface of workpieces such as three-dimensional complex curved surfaces, inner and outer walls of circles and dark grooves. During the processing, magnetic abrasives are first added to the processing area. Then, the abrasives will be linked along the direction of the magnetic lines of force under the action of the magnetic field to form an abrasive brush (FMAB) with a certain rigidity that is pressed on the surface of the workpiece. When the workpiece and the magnetic pole move relative to each other, the abrasive brush is like a flexible tool that rubs and scratches the surface of the workpiece, thereby removing a small amount of material and reducing the surface roughness. As the "tool" in the processing process, the grinding performance and service life of the magnetic abrasive will directly affect the efficiency of magnetic abrasive processing and the quality of surface finishing.
[0003] At present, the preparation of magnetic abrasives in my country is still in the experimental research stage, mainly using simple mixing method, sintering method, bonding method, atomization rapid solidification method, etc., there are still problems such as high preparation cost, insufficient sphericity, poor self-sharpening and low service life. Therefore, there is an urgent need to develop new magnetic abrasives with stable structure and long service life. Summary of the invention
[0004] The object of the present invention is to provide a magnetic abrasive and a preparation method thereof, so as to solve the problems of insufficient service life, low sphericity and poor self-sharpening of the magnetic abrasive mentioned in the above background technology.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A magnetic abrasive, comprising a ferromagnetic phase matrix and an abrasive phase grinding layer wrapped on the surface of the ferromagnetic phase matrix, wherein the ferromagnetic phase matrix is composed of magnetic functional components, and the abrasive phase grinding layer is a hard diffusion infiltration layer distributed in a gradient along the radial direction of the ferromagnetic phase matrix, so that a multi-layer core-shell structure is formed in the magnetic abrasive.
[0007] Optionally, the magnetic functional component is Fe, and the abrasive phase grinding layer includes an inner diffusion layer, an intermediate diffusion layer and an outer diffusion layer, the inner diffusion layer is a Fe2B layer, the intermediate diffusion layer is a FeB layer, and the outer diffusion layer is a FeB layer mixed with B4C.
[0008] Optionally, the abrasive phase grinding layer has a thickness of 32-38 μm.
[0009] Optionally, the average particle size of the ferromagnetic phase matrix is 200 μm-300 μm.
[0010] A method for preparing a magnetic abrasive, wherein the magnetic abrasive is prepared by an embedding infiltration method, comprising the following steps:
[0011] (1) preparing a penetrant by mixing a ferromagnetic phase matrix, a material to be infiltrated, and a catalyst according to a preset mass percentage;
[0012] (2) The penetrant is subjected to a thermal diffusion penetrating treatment to obtain the magnetic abrasive.
[0013] Optionally, in step (1), the catalyst is KBF4, the material to be infiltrated is B4C, the ferromagnetic phase matrix is Fe, and the mass percentages are: 10-15wt.% KBF4, 50-55wt.% B4C, 30-40wt.% Fe.
[0014] Optionally, a star ball mill is used to uniformly mix the penetrant; wherein the mixing time is 20 minutes.
[0015] Optionally, in step (1), after the penetrant is prepared, the process further includes sealing the penetrant with an alumina crucible; wherein, when there are gaps in the alumina crucible, the filler added is Al2O3, and the standing time after sealing the alumina crucible with the sealant is 1.5h-2h.
[0016] Optionally, in step (2), a box-type resistance furnace is used to perform thermal diffusion infiltration treatment on the infiltration agent; wherein the heating rate of the box-type resistance furnace is set to 10°C / min, the thermal diffusion infiltration temperature is set to 850°C, and the thermal diffusion infiltration insulation time is 2h.
[0017] Optionally, in step (2), after obtaining the magnetic abrasive, the method further includes air cooling, screening, washing and drying the magnetic abrasive.
[0018] The beneficial effects of the present invention are:
[0019] The magnetic abrasive of the present invention solves the technical problems of poor bonding, insufficient service life, low sphericity, poor self-sharpening and the like of the magnetic abrasive in the prior art, and achieves beneficial effects: the magnetic abrasive forms a uniform gradient diffusion layer with a metallurgical bonding interface on the surface of the ferromagnetic phase to achieve uniform coating of ferromagnetic phase particles; during the grinding process, when the outer grinding layer of the abrasive is broken or even partially peeled off due to wear, the new "knife edge" formed by the surface height difference of the residual outer layer and the exposed inner grinding layer after peeling off are both abrasive, which effectively improves the self-sharpening of the magnetic abrasive and prolongs its service life.
[0020] The preparation method of magnetic abrasive of the present invention solves the technical problems of high cost, complicated process, poor bonding and short life of the obtained magnetic abrasive in the prior art, and achieves beneficial effects: the preparation method generates a hard grinding "layer" on the surface of ferromagnetic phase particles in situ through an improved embedding infiltration process, so that each angle contact surface of the grinding layer has cutting properties, which is equivalent to evenly arranging a large number of cutting edges on the surface of the ferromagnetic phase to form a "blade shell", effectively improving the contact rate between the abrasive blade and the workpiece to be processed. At the same time, giving the abrasive a higher sphericity also makes the abrasive have better fluidity. Good fluidity will effectively promote the tumbling and replacement of the abrasive in the processing area, ensuring the continuous high-efficiency processing; in the initial stage of grinding, Thanks to the good interface bonding performance and high hardness of the abrasive grinding layer, the "notches" formed by a small amount of wear have little effect on the overall abrasiveness of the abrasive; in the middle stage of wear, the adjacent surface "notches" will be "connected" and gradually evolved into new "edges" with a "serrated" distribution. Its good self-sharpening property enables the grinding process to be carried out continuously and efficiently; in the late stage of wear, the grinding phases of the outer and middle layers of the abrasive are gradually "consumed", and the internal grinding layers exposed after peeling have grinding properties and will continue to participate in the subsequent grinding process, effectively improving the self-sharpening property of the magnetic abrasive and extending its service life (240 minutes); the process is simple, low-cost, and the magnetic abrasive produced has the characteristics of high performance and long life. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings in the specification, which constitute a part of this application, are used to provide a further understanding of the present invention. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0022] Figure 1 is a surface topography diagram of a magnetic abrasive provided according to an embodiment of the present invention;
[0023] Figure 2 yes Figure 1 The enlarged view of point A in the middle;
[0024] Figure 3 is a cross-sectional morphology diagram of a magnetic abrasive provided according to an embodiment of the present invention;
[0025] Figure 4 yes Figure 3 The enlarged view of point B in the middle;
[0026] Figure 5 is a process flow chart of a method for preparing a magnetic abrasive according to an embodiment of the present invention;
[0027] Figure 6 is an X-ray diffraction diagram of a magnetic abrasive provided according to an embodiment of the present invention;
[0028] Figure 7It is a wear schematic diagram of the grinding life experiment of the magnetic abrasive provided according to the embodiment of the present invention. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. The components of the embodiments of the present invention generally described and shown in the drawings here can be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents the selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present invention.
[0030] In the description of the embodiments of the present invention, it should be understood that the terms "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present invention.
[0031] Below, refer to Figure 1-6 A magnetic abrasive and a preparation method thereof according to an embodiment of the present invention are described in detail.
[0032] The surface topography can be used to observe the geometric shape and properties of the material surface, and the cross-sectional topography can be used to observe the thickness of the material cross section, such as Figure 1-4 As shown, a magnetic abrasive is provided according to an embodiment of the present invention, wherein the magnetic abrasive includes a ferromagnetic phase matrix and an abrasive phase grinding layer wrapped on the surface of the ferromagnetic phase matrix, wherein the component of the ferromagnetic phase matrix is a magnetic functional component, and the abrasive phase grinding layer is a hard diffusion layer gradiently distributed along the radial direction of the ferromagnetic phase matrix, so that a multi-layer core-shell structure is formed in the magnetic abrasive.
[0033] It should be noted that the hard diffusion layer has a metallurgical bonding interface; the distribution of the abrasive phase on the surface of the ferromagnetic phase, the bonding characteristics with the ferromagnetic phase, the protruding height of the abrasive, the shape, size, micromorphology and other properties of the abrasive determine the performance and life of the magnetic abrasive. Figure 1-4As shown, the surface of the magnetic abrasive is uniformly coated with a light gray "cauliflower-like" structure mixed with dark gray particles, and the prepared infiltration layer is dense and uniform, without obvious holes, cracks and peeling. The irregular morphology of dark gray particles (blade height 10.15μm) and light gray structure (blade height 6.25μm) and the "angle difference" formed by their uniform arrangement on the spherical surface make it "evolve" into the cutting edge of the abrasive surface, and the overall morphology is a spherical abrasive with high sphericity and uniform distribution of cutting edges. Therefore, the magnetic abrasive achieves uniform coating of ferromagnetic phase particles by forming a uniform gradient diffusion layer with a metallurgical bonding interface on the surface of the ferromagnetic phase. During the grinding process, when the external grinding layer of the abrasive is broken or even partially peeled off due to wear, the new "knife edge" formed by the surface height difference of the residual outer layer and the internal grinding layer exposed after peeling are both abrasive, which effectively improves the self-sharpening property of the magnetic abrasive and prolongs its service life.
[0034] like Figure 3-4 As shown, in one embodiment, the magnetic functional component is Fe, and the abrasive phase grinding layer includes an inner diffusion infiltration layer, an intermediate diffusion infiltration layer and an outer diffusion infiltration layer, wherein the inner diffusion infiltration layer is a Fe2B layer, the intermediate diffusion infiltration layer is a FeB layer, and the outer diffusion infiltration layer is a FeB layer mixed with B4C. It should be noted that Fe is more likely to have magnetism, and the high magnetic energy product and high coercive force of B make it an ideal material for making high-performance permanent magnets. Therefore, the present invention uses the Fe-B system, and the bonding of the magnetic abrasive can be improved at high temperature through the external diffusion of Fe matrix elements and the internal diffusion of the B elements to be infiltrated, so that the magnetic abrasive is not easy to decompose during the grinding process, thereby extending the life of the magnetic abrasive.
[0035] In one embodiment, the abrasive phase grinding layer has a thickness of 32-38 μm. It should be noted that, in this embodiment, preferably, the abrasive phase grinding layer has a thickness of 36.5 μm, wherein the inner diffusion layer has a thickness of 19.5 μm, the middle diffusion layer has a thickness of 9.7 μm, and the outer diffusion layer has a thickness of 7.3 μm. In this way, a sufficient number of abrasive particles can be ensured to maintain an efficient grinding rate, and problems such as increased thermal impact and increased surface roughness caused by an overly thick grinding layer can be avoided, thereby improving the grinding effect of the magnetic abrasive.
[0036] like Figure 1-2 As shown, in one embodiment, the average particle size of the ferromagnetic phase matrix is 200 μm-300 μm. It should be noted that in this embodiment, preferably, the particle size of the magnetic abrasive is 293.4 μm. Thus, it can be adsorbed on the surface of the magnetic pole or the magnetic control device / unit to form a flexible grinding brush, which can have better fluidity when finishing the workpiece surface.
[0037] like Figure 5 As shown, a method for preparing a magnetic abrasive, wherein the magnetic abrasive is prepared by an embedding infiltration method, comprises the following steps:
[0038] (1) preparing a penetrant by mixing a ferromagnetic phase matrix, a material to be infiltrated, and a catalyst according to a preset mass percentage;
[0039] (2) The penetrant is subjected to a thermal diffusion penetrating treatment to obtain the magnetic abrasive.
[0040] It should be noted that, in the present embodiment, preferably, the ferromagnetic phase matrix is a spherical powder; the embedding infiltration technology belongs to chemical vapor deposition (CVD), which is a relatively mature metal surface treatment technology that combines the advantages of simple operation, low cost, no influence on factors such as workpiece shape and size, strong repeatability, etc., and is widely used in the surface treatment of bulk materials; unlike other surface modification treatment technologies (spraying, PVD, laser modification), the embedding infiltration process is not affected by the workpiece size and shape factors, which becomes the key to breaking the barriers of other traditional surface modification treatment technologies in the surface modification of tiny ferromagnetic powders.
[0041] Therefore, the preparation method of the magnetic abrasive improves the embedding and infiltration process to generate a hard grinding "layer" in situ on the surface of the ferromagnetic phase particles, so that all angle contact surfaces of the grinding layer have cutting properties, which is equivalent to evenly arranging a large number of cutting edges on the ferromagnetic phase surface to form a "blade shell", effectively improving the contact rate between the abrasive blade and the workpiece. At the same time, giving the abrasive a higher sphericity also makes the abrasive have better fluidity. Good fluidity will effectively promote the tumbling and replacement of the abrasive in the processing area, ensuring the continuous high-efficiency processing, and achieving the characteristics of simple process, low cost and high performance and long life of the magnetic abrasive.
[0042] In one embodiment, in step (1), the catalyst is KBF4, the material to be infiltrated is B4C, the ferromagnetic phase matrix is Fe, and the mass percentages are: 10-15wt.% KBF4, 50-55wt.% B4C, 30-40wt.% Fe.
[0043] In this embodiment, the formation of the gradient grinding layer on the abrasive surface mainly relies on the interfacial diffusion reaction under high temperature. This process is usually manifested as the external diffusion of Fe matrix elements and the internal diffusion of B elements to be infiltrated. This process is controlled by the competitive adsorption of active atoms of the infiltrated elements on the alloy surface and the diffusion rate of atoms in the infiltrated layer. The overall reaction process mainly includes the gaseous reaction stage of the generation of active B atoms and its subsequent solid-state diffusion process.
[0044] In this embodiment, during the B infiltration process using KBF4 as a catalyst, KBF4 does not directly participate in the reaction, but dissociates to form halide vapor during the furnace heating process; then, B4C in the infiltrant will react with the generated halide vapor to generate gaseous halide; the generated gaseous halide will diffuse to the surface of the substrate under the action of the chemical potential gradient and decompose into active B atoms; the active B atoms will be preferentially adsorbed by the sites with high surface energy of the substrate alloy to participate in the subsequent solid-state diffusion process. In the early stage of solid-state diffusion reaction, the active B atoms in the infiltration bag will, driven by the chemical potential gradient, enter the interior of the Fe matrix along the channel for the outward diffusion of Fe atoms (EDS analysis was performed on samples taken from the infiltration agent adjacent to the sample surface after the experiment, and the results showed that the Fe content in the infiltration agent reached 3.36at.%, indicating that the Fe element in the matrix alloy diffused outward) and preferentially deposit to form Fe2B. On the other hand, they will directly react with the outward-diffused Fe atoms at the surface interface of the matrix to form a B-rich FeB phase outer layer. This process will inevitably include a small amount of B4C powder to be infiltrated in the infiltration bag, which is manifested as sporadic distribution of B4C particles in the surface morphology of the abrasive. As the diffusion reaction continues, the Fe2B preferentially deposited will gradually transform into the FeB phase as the content of the internally diffused B increases, forming an intermediate layer of the infiltration layer, while the Fe2B preferentially generated by the internal diffusion and not undergoing phase transformation forms the inner layer of the infiltration layer, and finally a multi-layer core-shell magnetic abrasive with an FeB outer layer, a FeB intermediate layer and a Fe2B inner layer with B4C particles included is obtained.
[0045] In the present embodiment, preferably, Fe is spherical Fe powder (purity ≥99%) prepared by atomization method, with an average particle size between 200-300 μm and good sphericity; in the present embodiment, preferably, B4C is B4C powder (AR grade, purity ≥99%), with an average particle size of about 5 μm; in the present embodiment, preferably, KBF4 uses Sinopharm KBF4 reagent (AR grade, purity ≥99%).
[0046] It should be noted that the inventors finally determined the appropriate raw material ratio range for preparing the magnetic abrasive through a large number of repeated experiments and screenings and a series of creative work.
[0047] Thereby, the beneficial effects of the obtained magnetic abrasive are further improved.
[0048] In one embodiment, a planetary ball mill is used to uniformly mix the penetrant, wherein the mixing time is 20 minutes. Thus, the components can be mixed conveniently and fully to obtain a uniform grinding phase grinding layer.
[0049] In one embodiment, in step (1), after the penetrant is prepared, the process further includes sealing the penetrant with an alumina crucible; wherein the filler added when there is a gap in the alumina crucible is Al2O3, and the standing time after the alumina crucible is sealed with the sealant is 1.5h-2h. It should be noted that the filler Al2O3 does not participate in the reaction, but only makes the alumina crucible an oxygen-free environment; the standing time is set to ensure that the sealant is completely dry; thus, in an oxygen-free environment, the penetrant can be protected and heat-treated.
[0050] In one embodiment, in step (2), a box-type resistance furnace is used to perform thermal diffusion infiltration treatment on the infiltrant; wherein the box-type resistance furnace heating rate is set to 10°C / min, the thermal diffusion infiltration temperature is set to 850°C, and the thermal diffusion infiltration holding time is 2h. It should be noted that the inventors have also finally determined the thermal diffusion infiltration treatment conditions for the infiltrant through a large number of repeated experiments and screenings, and through a series of creative labor, thereby further improving and optimizing the beneficial effects of the above-mentioned magnetic abrasive.
[0051] In one embodiment, in step (2), after obtaining the magnetic abrasive, the process further includes air cooling, screening, washing and drying the magnetic abrasive, thereby removing impurities, such as filler Al2O3, and obtaining the magnetic abrasive with better effect and purer quality.
[0052] The magnetic abrasive and the preparation method thereof of the present invention are further described below in conjunction with specific embodiments.
[0053] Example 1
[0054] A magnetic abrasive comprises a ferromagnetic phase matrix and an abrasive phase grinding layer wrapped on the surface of the ferromagnetic phase matrix, the ferromagnetic phase matrix is composed of Fe, the abrasive phase grinding layer is a Fe-B intermetallic compound hard diffusion infiltration layer distributed in a gradient along the radial direction of the ferromagnetic phase matrix, the abrasive phase grinding layer comprises a multilayer core-shell structure of an inner diffusion infiltration layer, an intermediate diffusion infiltration layer and an outer diffusion infiltration layer, the inner diffusion infiltration layer is a Fe2B layer, the intermediate diffusion infiltration layer is a FeB layer, and the outer diffusion infiltration layer is a FeB layer interspersed with B4C.
[0055] Example 2
[0056] A method for preparing a magnetic abrasive:
[0057] (1) KBF4, B4C powder and Fe spherical powder were mixed according to a preset mass percentage of 10wt.% KBF4, 55wt.% B4C, and 35wt.% Fe, and then placed in a star ball mill for uniform mixing for 20 minutes to obtain a penetrant; the penetrant was poured into an alumina crucible, and Al2O3 filler was added to ensure an oxygen-free environment inside the alumina crucible, and an appropriate amount of sealant was taken to seal the crucible, and then it was left to stand at room temperature for 1.5 hours to ensure that the binder was dry;
[0058] (2) placing a sealed alumina crucible in a box-type resistance furnace, setting the heating rate of the box-type resistance furnace to 10°C / min, the thermal diffusion temperature to 850°C, and the thermal diffusion insulation time to 2h to obtain the magnetic abrasive; air-cooling the magnetic abrasive, sieving, ultrasonically cleaning with acetone, and drying.
[0059] Example 3
[0060] A method for preparing a magnetic abrasive:
[0061] (1) KBF4, B4C powder and Fe spherical powder were mixed according to a preset mass percentage of 15wt.% KBF4, 50wt.% B4C, and 35wt.% Fe, and then placed in a star ball mill for uniform mixing for 20 minutes to obtain a penetrant; the penetrant was poured into an alumina crucible, and Al2O3 filler was added to ensure an oxygen-free environment inside the alumina crucible, and an appropriate amount of sealant was taken to seal the crucible, and then it was left to stand at room temperature for 1.5 hours to ensure that the binder was dry;
[0062] (2) placing a sealed alumina crucible in a box-type resistance furnace, setting the heating rate of the box-type resistance furnace to 10°C / min, the thermal diffusion temperature to 850°C, and the thermal diffusion insulation time to 2h to obtain the magnetic abrasive; air-cooling the magnetic abrasive, sieving, ultrasonically cleaning with acetone, and drying.
[0063] Example 4
[0064] A method for preparing a magnetic abrasive:
[0065] (1) KBF4, B4C powder and Fe spherical powder were mixed according to a preset mass percentage of 10wt.% KBF4, 50wt.% B4C, and 40wt.% Fe, and then placed in a planetary ball mill for uniform mixing for 20 minutes to obtain a penetrant; the penetrant was poured into an alumina crucible, and Al2O3 filler was added to ensure an oxygen-free environment inside the alumina crucible, and an appropriate amount of sealant was taken to seal the crucible, and then it was left to stand at room temperature for 2 hours to ensure that the binder was dry;
[0066] (2) placing a sealed alumina crucible in a box-type resistance furnace, setting the heating rate of the box-type resistance furnace to 10°C / min, the thermal diffusion temperature to 850°C, and the thermal diffusion insulation time to 2h to obtain the magnetic abrasive; air-cooling the magnetic abrasive, sieving, ultrasonically cleaning with acetone, and drying.
[0067] Example 5
[0068] A method for preparing a magnetic abrasive:
[0069] (1) KBF4, B4C powder and Fe spherical powder were mixed according to a preset mass percentage of 15wt.% KBF4, 55wt.% B4C, and 30wt.% Fe, and then placed in a planetary ball mill for uniform mixing for 20 minutes to obtain a penetrant; the penetrant was poured into an alumina crucible, and Al2O3 filler was added to ensure an oxygen-free environment inside the alumina crucible, and an appropriate amount of sealant was taken to seal the crucible, and then it was left to stand at room temperature for 2 hours to ensure that the binder was dry;
[0070] (2) placing a sealed alumina crucible in a box-type resistance furnace, setting the heating rate of the box-type resistance furnace to 10°C / min, the thermal diffusion temperature to 850°C, and the thermal diffusion insulation time to 2h to obtain the magnetic abrasive; air-cooling the magnetic abrasive, sieving, ultrasonically cleaning with acetone, and drying.
[0071] Example 6
[0072] A method for preparing a magnetic abrasive:
[0073] (1) KBF4, B4C powder and Fe spherical powder were mixed according to a preset mass percentage of 13wt.% KBF4, 53wt.% B4C, and 34wt.% Fe, and then placed in a planetary ball mill for uniform mixing for 20 minutes to obtain a penetrant; the penetrant was poured into an alumina crucible, and Al2O3 filler was added to ensure an oxygen-free environment inside the alumina crucible, and an appropriate amount of sealant was taken to seal the crucible, and then it was left to stand at room temperature for 1.5 hours to ensure that the binder was dry;
[0074] (2) placing a sealed alumina crucible in a box-type resistance furnace, setting the heating rate of the box-type resistance furnace to 10°C / min, the thermal diffusion temperature to 850°C, and the thermal diffusion insulation time to 2h to obtain the magnetic abrasive; air-cooling the magnetic abrasive, sieving, ultrasonically cleaning with acetone, and drying.
[0075] X-ray diffraction patterns play an important role in the fields of materials science, chemistry, physics, etc. They are mainly used to study the crystal structure of substances, including determining the crystal structure of substances, measuring lattice parameters and grain size. Energy spectrometers are used to analyze the types and contents of the elements in the micro-regions of materials, in conjunction with scanning electron microscopes and transmission electron microscopes. Figure 6 As shown, the magnetic abrasive is analyzed by using X-ray diffraction technology and energy spectrometer, and the X-ray diffraction spectrum and energy spectrometer point scanning results indicate that the dark gray particles and light gray structure are B4C and FeB phases, respectively, and the two are evenly distributed.
[0076] like Figure 7 As shown, the grinding life test of the magnetic abrasive is carried out, and the test method is to carry out a magnetic grinding processing experiment on a titanium alloy pipe, and the time until the abrasive loses its grinding effect is determined as the grinding life of the abrasive. The experiment shows that during the grinding process of the abrasive with a multi-layer core-shell structure, the gradient hard phase on the surface inevitably wears, breaks, or even peels off. In the early stage of wear (60 minutes of grinding), due to the uniform distribution of the grinding phase on the abrasive surface and the excellent fluidity brought by its high sphericity, the "notches" formed by a small amount of wear have little effect on the overall abrasiveness of the abrasive; in the middle stage of wear (120 minutes to 180 minutes of grinding), the adjacent surface "notches" will be "connected" and gradually evolved into new "edges" with a "serrated" distribution. Its good self-sharpening property enables the grinding process to be carried out continuously and efficiently; in the late stage of wear (210 minutes to 270 minutes of grinding), the grinding phases of the outer and middle layers of the abrasive are gradually "consumed", and the exposed inner hard phases after peeling will continue to participate in the subsequent grinding process to further extend the service life of the abrasive. Therefore, before the internal grinding layer is completely peeled off, the abrasive can produce a certain cutting effect.
[0077] After the sample titanium tube was processed three times with the magnetic abrasive after grinding for 150 minutes, the improvement of the surface roughness of the titanium tube by the original abrasive was only 15.16% higher than that by the abrasive after grinding for 150 minutes. Figure 7 The surface morphology of the abrasive after grinding for 270 minutes shows that the effective life of the abrasive is about 240 minutes. The gradient hard layer magnetic abrasive prepared by the present invention prolongs its service life through the wear and replacement of the gradient grinding layer, and has excellent durability.
[0078] In the description of this specification, the description with reference to the terms "one embodiment", "one example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine different embodiments or examples described in this specification and the features of different embodiments or examples without contradiction.
[0079] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A magnetic abrasive, characterized in that: The magnetic abrasive comprises a ferromagnetic phase matrix and an abrasive phase grinding layer wrapped on the surface of the ferromagnetic phase matrix. The component of the ferromagnetic phase matrix is a magnetic functional component, and the abrasive phase grinding layer is a hard diffusion layer distributed in a gradient along the radial direction of the ferromagnetic phase matrix, so that a multi-layer core-shell structure is formed in the magnetic abrasive.
2. The magnetic abrasive according to claim 1, characterized in that: The magnetic functional component is Fe, and the abrasive phase grinding layer includes an inner diffusion layer, an intermediate diffusion layer and an outer diffusion layer. The inner diffusion layer is a Fe2B layer, the intermediate diffusion layer is a FeB layer, and the outer diffusion layer is a FeB layer mixed with B4C.
3. The magnetic abrasive according to claim 1, characterized in that: The abrasive phase grinding layer has a thickness of 32-38 μm.
4. The magnetic abrasive according to claim 1, characterized in that: The average particle size of the ferromagnetic phase matrix is 200 μm-300 μm.
5. A method for preparing a magnetic abrasive, characterized in that: The magnetic abrasive is prepared by an embedding infiltration method, comprising the following steps: (1) preparing a penetrant by mixing a ferromagnetic phase matrix, a material to be infiltrated, and a catalyst according to a preset mass percentage; (2) The penetrant is subjected to a thermal diffusion penetrating treatment to obtain the magnetic abrasive.
6. The method for preparing a magnetic abrasive according to claim 5, characterized in that: In step (1), the catalyst is KBF4, the material to be infiltrated is B4C, the ferromagnetic phase matrix is Fe, and the mass percentages are: 10-15wt.% KBF4, 50-55wt.% B4C, and 30-40wt.% Fe.
7. The method for preparing a magnetic abrasive according to claim 5, characterized in that: In step (1), a planetary ball mill is used to uniformly mix the penetrant; wherein the mixing time is 20 minutes.
8. The method for preparing a magnetic abrasive according to claim 5, characterized in that: In step (1), after the penetrant is prepared, the method further includes sealing the penetrant with an alumina crucible; wherein, when there are gaps in the alumina crucible, the filler added is Al2O3, and the standing time after the alumina crucible is sealed with a sealant is 1.5h-2h.
9. The method for preparing a magnetic abrasive according to claim 5, characterized in that: In step (2), a box-type resistance furnace is used to perform thermal diffusion treatment on the penetrant; wherein the heating rate of the box-type resistance furnace is set to 10°C / min, the thermal diffusion temperature is set to 850°C, and the thermal diffusion insulation time is 2h.
10. The method for preparing magnetic abrasive according to claim 5, characterized in that: In step (2), after obtaining the magnetic abrasive, the method further includes air cooling, screening, washing and drying the magnetic abrasive.