Easily disintegrated soil conditioner as well as preparation method and application thereof
By preparing the mixing and granulation technology of silica-rich substances with appropriate SiO2 content and activator, the problem of long dissolution time and poor disintegration effect of soil conditioners is solved, and the rapid disintegration and effective ingredients of soil conditioners are achieved. The release of products improves the convenience and timeliness of the product.
Patent Information
- Application Number
- CN202310597829.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
The existing soil conditioning agents dissolve for too long during use, which affects the convenience and timeliness of the product. The disintegration effect of the granular product has not been effectively paid attention to, and dust-induced effects are easily produced when applied to powdered products.
Silica-rich substances with SiO2 content of 55-80 wt% were mixed with an activator, and then activated and crushed after adding water to form, and an appropriate amount of binder was added to granulate to prepare a granular soil conditioner that was easily disintegrated.
The prepared soil conditioner not only quickly disintegrates and releases active ingredients in water, improves the convenience and age of the product, but also meets strength requirements and avoids the potential harm of the binder to soil and plants.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of soil conditioners and relates to an easily disintegratable soil conditioner and a preparation method and application thereof. Background Art
[0002] At present, there have been many studies on the preparation and application of soil conditioners. Silicon-containing soil conditioners can not only adjust the soil pH value and passivate heavy metals to achieve the purpose of improving soil, but also provide crops with the nutrient element silicon required for growth, so as to improve the crop's ability to resist pests and diseases, drought and waterlogging, and improve crop yields and agricultural product quality. Currently, most soil conditioners are in powder form, and powdered soil conditioners will produce dust when applied, affecting the effect. The granular soil conditioners currently prepared are generally granulated by adding binders to the powdered products produced, but current reports often only focus on the bonding effect of binders on soil conditioners, ignoring the disintegration effect of granular finished soil conditioners, and often do not pay attention to the content of active ingredients in soil conditioners. If the soil conditioner takes too long to dissolve during use, it will affect the convenience and timeliness of the product.
[0003] CN 113817474A discloses an acidic soil conditioner and a preparation method thereof, wherein potassium-containing minerals, calcium-containing minerals and zeolite are mixed in proportion, roasted at high temperature for a certain period of time, cooled, ground and sieved to obtain the acidic soil conditioner. The prepared acidic soil conditioner is a powdery soil conditioner.
[0004] CN 106244148A discloses a process for producing a soil conditioner using waste from a steel plant, wherein waste limestone powder and dolomite powder produced by the steel plant are mixed with ground potassium feldspar powder, 5% bentonite is added as a binder after mixing, and pelletization is performed to make it a citric acid-soluble soil conditioner. The content of the main active ingredient of the prepared granular soil conditioner is not given, and the disintegration effect of the granular product is not mentioned.
[0005] CN 113248333A discloses a granular soil conditioner for composite heavy metal pollution and a preparation method thereof, wherein biomass charcoal, sodium selenite, desulfurized gypsum, lignite and wollastonite are mixed in proportion, granulated, dried and passed through a 10-mesh sieve to obtain the granular soil conditioner. The disintegration effect of the prepared granular soil conditioner is unknown. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention provides a method for preparing an easily disintegrating soil conditioner, comprising the following steps:
[0007] (1) mixing a silicon dioxide-rich material having a SiO2 content of 55-80 wt% (e.g., 55 wt%, 56 wt%, 57 wt%, 58 wt%, 59 wt%, 60 wt%, 61 wt%, 62 wt%, 63 wt%, 64 wt%, 65 wt%, 66 wt%, 67 wt%, 68 wt%, 69 wt%, 70 wt%, 71 wt%, 72 wt%, 73 wt%, 74 wt%, 75 wt%, 76 wt%, 77 wt%, 78 wt%, 79 wt%, 80 wt%, or the content in the range and value between any two of these values) and an activator, adding water to form a granular raw material;
[0008] (2) activating the granular raw material to obtain an activated granular raw material;
[0009] (3) crushing the activated granular raw material to obtain a powdered soil conditioner;
[0010] (4) The powdered soil conditioner and the binder are mixed and granulated to obtain an easily disintegrable granular soil conditioner.
[0011] In some embodiments, in the above method, in step (1), the silicon dioxide-rich material is selected from one or more of fly ash, coal gangue, fly ash acid aluminum extraction residue, and coal gasification slag, as long as the SiO2 content is 55-80wt%.
[0012] In some embodiments, in any of the above methods, in step (1), the activator is selected from one or more of calcium oxide, calcium hydroxide, potassium carbonate, potassium hydroxide, sodium carbonate, magnesium oxide, brucite, and talc, preferably a combined activator comprising two or more of them, more preferably a combined activator consisting of calcium hydroxide and sodium carbonate, further preferably a combined activator consisting of calcium hydroxide and sodium carbonate in a mass ratio of calcium hydroxide to sodium carbonate of 1:(0.18-1), and the activator can provide elements such as calcium, potassium and / or magnesium required for crop growth.
[0013] In some embodiments, in any of the above methods, in step (1), the mass ratio of the silica-rich material to the activator is 1:(0.7-1).
[0014] In some embodiments, in any of the above methods, in step (1), the molding method is extrusion molding or pelletizing molding, and any extrusion or pelletizing method known in the art can be used.
[0015] In some embodiments, in any of the above methods, the volume of the granular raw material is no greater than 4 cm 3 , preferably no larger than 3cm 3, for example, it can be 1cm 3 , 2cm 3 , 3cm 3 , or the volume shown by the range and value between any two of these values.
[0016] In some embodiments, in any of the above methods, in step (2), the activation conditions are: activation temperature 600-950°C (for example, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, or the temperature indicated by the range and value between any two of these values), activation time 0.5-3h (for example, 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, or the time indicated by the range and value between any two of these values);
[0017] There can also be a drying step before activation, such as drying, and the drying conditions can be: a drying temperature of 30-80°C (for example, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, or the temperature shown in the range and numerical value between any two of these values), and a drying time of 3-12h (for example, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, or the time shown in the range and numerical value between any two of these values).
[0018] In some embodiments, in any of the above methods, in step (3), the powdered soil conditioner has a particle size of less than 200 meshes and can be pulverized by any pulverization method known in the art, such as pulverizing by a high-speed pulverizer.
[0019] In some embodiments, in any of the methods described above, in step (4), the binder is selected from one or more of sodium humate, desulfurized gypsum, α-starch, and attapulgite, and the added amount is 0.5-8% of the mass of the powdered soil conditioner (for example, 0.5%, 1%, 2%, 4%, 6%, 8%, or the content shown in the range and value between any two of these values). The addition of this binder can not only improve the molding efficiency and make the strength of the finished granules meet the requirements, but also can act as a disintegrant, so that the finished granules can quickly disintegrate when exposed to water, which is helpful for plants to absorb and utilize.
[0020] In some embodiments, in any of the methods described above, the particle size of the granular soil conditioner is 2-5 mm, for example, it can be 2 mm, 2.5 mm, 3 mm, 3.5 mm, 4 mm, 4.5 mm, 5 mm, or the range and value between any two of these values.
[0021] The present invention also provides a soil conditioner prepared by any of the above methods.
[0022] The present invention also provides the use of the soil conditioner in improving soil and / or as soil fertilizer.
[0023] The beneficial effects of the present invention are as follows:
[0024] (1) The soil conditioner prepared by the present invention can not only improve the soil, but also provide beneficial elements such as silicon and calcium required for crop growth as silicon fertilizer;
[0025] (2) The granular product can quickly disintegrate in water while meeting the strength requirements, thus promoting the release of the active ingredients;
[0026] (3) The addition of binders / disintegrants will not introduce harmful elements that may harm the soil or plants;
[0027] (4) The amount of binder / disintegrant added is small and will not change the general chemical composition of the soil conditioner. DETAILED DESCRIPTION
[0028] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0029] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0030] The present invention will be further described below in conjunction with specific examples. It should be understood that the following examples are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0031] The silicon content is determined according to NY / T 2272-2012 “Determination of calcium, magnesium and silicon content of soil conditioners”.
[0032] The fly ash acid-process aluminum extraction residue is the residue obtained by the fly ash through the hydrochloric acid acid dissolution process to extract aluminum.
[0033] According to the industry standard NY / T 797-2004 "Silicon Fertilizer", the effective silicon content (measured in SiO2) of qualified silicon fertilizer is above 20wt%.
[0034] The strength is measured according to HG 2224-91 "Determination of average compressive strength of granular heavy superphosphate particles".
[0035] The disintegration time was measured by a disintegration instrument (Tianjin Tianfa Analytical Instrument Co., Ltd., BJ02 Intelligent Disintegration Instrument). The product particles were placed in a hanging basket, and the disintegration instrument was started for detection. The time for the particles to disintegrate and completely pass through the mesh was recorded. The mesh aperture of the hanging basket was 1 mm.
[0036] Example 1
[0037] (1) Accurately weigh dry fly ash acid aluminum extraction residue (SiO2 content is 65wt%), calcium hydroxide and sodium carbonate in a mass ratio of 1:0.48:0.4, mix them evenly, add water to form pellets, and prepare a volume of 2cm 3 of granular raw materials.
[0038] (2) The granular raw material obtained in step (1) is dried at 30° C. for 6 h, and then activated at 800° C. for 1.5 h. After cooling, an activated granular raw material is obtained.
[0039] (3) Grinding the activated granular raw material obtained in step (2) to a size of less than 200 meshes using a high-speed pulverizer to obtain a powdered soil conditioner.
[0040] (4) The powdered soil conditioner obtained in step (3) is mixed evenly with α-starch and then granulated, wherein the mass of α-starch is 1% of the mass of the powdered soil conditioner, and the particle size of the granulated product is 3.5 mm. After drying, an easily disintegratable granular soil conditioner can be obtained.
[0041] After testing, the effective silicon (in terms of SiO2) content of the obtained granular soil conditioner is 30.4wt%, which meets the standard of NY / T797-2004 "Silicon Fertilizer"; the strength is 60N, and the disintegration time is 7min 20s.
[0042] Example 2
[0043] (1) Accurately weigh dry fly ash acid-process aluminum extraction residue (SiO2 content is 65wt%), calcium hydroxide and sodium carbonate in a mass ratio of 1:0.6:0.2, mix them evenly, add water to form pellets, and prepare a volume of 3cm 3 granular raw materials.
[0044] (2) The granular raw material obtained in step (1) is dried at 45° C. for 4 h, and then activated at 850° C. for 2 h. After cooling, an activated granular raw material is obtained.
[0045] (3) Grinding the activated granular raw material obtained in step (2) to a size of less than 200 meshes using a high-speed pulverizer to obtain a powdered soil conditioner.
[0046] (4) The powdered soil conditioner obtained in step (3) is evenly mixed with sodium humate and then granulated, wherein the mass of the sodium humate is 8% of the mass of the powdered soil conditioner, and the particle size of the granulated product is 3 mm. After drying, an easily disintegratable granular soil conditioner can be obtained.
[0047] After testing, the effective silicon (in terms of SiO2) content of the obtained granular soil conditioner is 25.8wt%, which meets the standard of NY / T797-2004 "Silicon Fertilizer"; the strength is 22N and the disintegration time is 42s.
[0048] Example 3
[0049] (1) Accurately weigh dry fly ash acid-process aluminum extraction residue (SiO2 content is 65wt%), calcium hydroxide and sodium carbonate in a mass ratio of 1:0.8:0.15, mix them evenly, add water to form pellets, and prepare a volume of 3cm 3 granular raw materials.
[0050] (2) The granular raw material obtained in step (1) is dried at 60° C. for 3 h, and then activated at 920° C. for 3 h. After cooling, an activated granular raw material is obtained.
[0051] (3) Grinding the activated granular raw material obtained in step (2) to a size of less than 200 meshes using a high-speed pulverizer to obtain a powdered soil conditioner.
[0052] (4) The powdered soil conditioner obtained in step (3) is mixed evenly with desulfurized gypsum and then granulated, wherein the mass of the desulfurized gypsum is 4% of the mass of the powdered soil conditioner, and the particle size of the granulated product is 2 mm. After drying, an easily disintegratable granular soil conditioner can be obtained.
[0053] After testing, the obtained granular soil conditioner has an effective silicon content (in terms of SiO2) of 24.7wt%, which meets the standard of NY / T797-2004 "Silicon Fertilizer"; the strength is 14N, and the disintegration time is 3h 42min.
[0054] Example 4
[0055] (1) Accurately weigh dry fly ash acid-process aluminum extraction residue (SiO2 content is 60wt%), calcium hydroxide and sodium carbonate in a mass ratio of 1:0.51:0.19, mix them evenly, add water to form pellets, and prepare a volume of 3cm 3 granular raw materials.
[0056] (2) The granular raw material obtained in step (1) is dried at 60° C. for 3 h, and then activated at 950° C. for 3 h. After cooling, an activated granular raw material is obtained.
[0057] (3) Grinding the activated granular raw material obtained in step (2) to a size of less than 200 meshes using a high-speed pulverizer to obtain a powdered soil conditioner.
[0058] (4) The powdered soil conditioner obtained in step (3) is mixed evenly with attapulgite and then granulated, wherein the mass of the attapulgite is 8% of the mass of the powdered soil conditioner, and the particle size of the granulated product is 2 mm. After drying, an easily disintegratable granular soil conditioner can be obtained.
[0059] The test showed that the effective silicon (in terms of SiO2) content of the obtained granular soil conditioner was 22.5wt%, reaching the standard of NY / T797-2004 "Silicon Fertilizer"; the strength was 16N, and the disintegration time was 2h 36min.
[0060] Example 5
[0061] (1) Accurately weigh dry fly ash acid-process aluminum extraction residue (SiO2 content is 70wt%), calcium hydroxide and sodium carbonate in a mass ratio of 1:0.5:0.5, mix them evenly, add water to form pellets, and prepare a volume of 3cm 3 granular raw materials.
[0062] (2) The granular raw material obtained in step (1) is dried at 60° C. for 3 h, and then activated at 600° C. for 3 h. After cooling, an activated granular raw material is obtained.
[0063] (3) Grinding the activated granular raw material obtained in step (2) to a size of less than 200 meshes using a high-speed pulverizer to obtain a powdered soil conditioner.
[0064] (4) The powdered soil conditioner obtained in step (3) is mixed evenly with α-starch and then granulated, wherein the mass of α-starch is 0.5% of the mass of the powdered soil conditioner, and the particle size of the granulated product is 2 mm. After drying, an easily disintegratable granular soil conditioner can be obtained.
[0065] The test showed that the effective silicon (in terms of SiO2) content of the obtained granular soil conditioner was 20.4wt%, reaching the standard of NY / T797-2004 "Silicon Fertilizer"; the strength was 14N, and the disintegration time was 6min 56s.
[0066] Example 6
[0067] (1) Accurately weigh dry fly ash acid-process aluminum extraction residue (SiO2 content is 80wt%), calcium hydroxide and sodium carbonate in a mass ratio of 1:0.7:0.3, mix them evenly, add water to form pellets, and prepare a volume of 1cm 3 granular raw materials.
[0068] (2) The granular raw material obtained in step (1) is dried at 45° C. for 4 h, and then activated at 950° C. for 0.5 h. After cooling, an activated granular raw material is obtained.
[0069] (3) Grinding the activated granular raw material obtained in step (2) to a size of less than 200 meshes using a high-speed pulverizer to obtain a powdered soil conditioner.
[0070] (4) The powdered soil conditioner obtained in step (3) is evenly mixed with sodium humate and then granulated, wherein the mass of the sodium humate is 6% of the mass of the powdered soil conditioner, and the particle size of the granulated product is 3 mm. After drying, an easily disintegratable granular soil conditioner can be obtained.
[0071] After testing, the effective silicon (in terms of SiO2) content of the obtained granular soil conditioner is 26.2wt%, which meets the standard of NY / T797-2004 "Silicon Fertilizer"; the strength is 18N and the disintegration time is 56s.
[0072] Example 7
[0073] (1) Accurately weigh dry fly ash acid-process aluminum extraction residue (SiO2 content is 55wt%), calcium hydroxide and sodium carbonate in a mass ratio of 1:0.54:0.3, mix them evenly, add water to form pellets, and prepare a volume of 3cm 3 granular raw materials.
[0074] (2) The granular raw material obtained in step (1) is dried at 45° C. for 4 h, and then activated at 860° C. for 1 h. After cooling, an activated granular raw material is obtained.
[0075] (3) Grinding the activated granular raw material obtained in step (2) to a size of less than 200 meshes using a high-speed pulverizer to obtain a powdered soil conditioner.
[0076] (4) The powdered soil conditioner obtained in step (3) is evenly mixed with sodium humate and then granulated, wherein the mass of the sodium humate is 6% of the mass of the powdered soil conditioner, and the particle size of the granulated product is 3 mm. After drying, an easily disintegratable granular soil conditioner can be obtained.
[0077] After testing, the effective silicon (in terms of SiO2) content of the obtained granular soil conditioner is 27.9wt%, which meets the standard of NY / T797-2004 "Silicon Fertilizer"; the strength is 17N and the disintegration time is 49s.
[0078] Example 8
[0079] (1) Accurately weigh dry coal gangue (SiO2 content of 59 wt%), calcium hydroxide and sodium carbonate in a mass ratio of 1:0.58:0.21, mix them evenly, add water to form pellets, and prepare a volume of 2 cm 3 granular raw materials.
[0080] (2) The granular raw material obtained in step (1) is dried at 60° C. for 4 h, and then activated at 850° C. for 2 h. After cooling, an activated granular raw material is obtained.
[0081] (3) Grinding the activated granular raw material obtained in step (2) to a size of less than 200 meshes using a high-speed pulverizer to obtain a powdered soil conditioner.
[0082] (4) The powdered soil conditioner obtained in step (3) is evenly mixed with sodium humate and then granulated, wherein the mass of the sodium humate is 6% of the mass of the powdered soil conditioner, and the particle size of the granulated product is 3 mm. After drying, an easily disintegratable granular soil conditioner can be obtained.
[0083] After testing, the effective silicon (in terms of SiO2) content of the obtained granular soil conditioner is 21.02wt%, which meets the standard of NY / T797-2004 "Silicon Fertilizer"; the strength is 14N and the disintegration time is 47s.
[0084] Example 9
[0085] (1) Dry fly ash (SiO2 content: 64 wt%), calcium hydroxide and sodium carbonate in a mass ratio of 1:0.63:0.23 were accurately weighed, mixed evenly, and granulated into a volume of 1 cm by adding water. 3 granular raw materials.
[0086] (2) The granular raw material obtained in step (1) is dried at 45° C. for 4 h, and then activated at 860° C. for 1.5 h. After cooling, an activated granular raw material is obtained.
[0087] (3) Grinding the activated granular raw material obtained in step (2) to a size of less than 200 meshes using a high-speed pulverizer to obtain a powdered soil conditioner.
[0088] (4) The powdered soil conditioner obtained in step (3) is evenly mixed with sodium humate and then granulated, wherein the mass of the sodium humate is 6% of the mass of the powdered soil conditioner, and the particle size of the granulated product is 3 mm. After drying, an easily disintegratable granular soil conditioner can be obtained.
[0089] After testing, the obtained granular soil conditioner has an effective silicon content (in terms of SiO2) of 23.80wt%, which meets the standard of NY / T797-2004 "Silicon Fertilizer"; the strength is 13N, and the disintegration time is 50s.
[0090] The present invention has been described with reference to the embodiments and examples. However, the present invention is not limited to the aspects described in the above embodiments and examples, and various modifications may be made. It should be understood that it is possible for those skilled in the art to make various modifications and equivalent substitutions to the present invention without departing from the spirit and scope of the present invention. Therefore, the present invention is not limited to the specific embodiments described herein. More specifically, the scope of protection of the present invention is defined by the appended claims.
Claims
1. A method for preparing an easily disintegrating soil conditioner, comprising the following steps: (1) mixing a silicon dioxide-rich material having a SiO2 content of 55-80 wt% and an activator, adding water to form a granular raw material; (2) activating the granular raw material to obtain an activated granular raw material; (3) crushing the activated granular raw material to obtain a powdered soil conditioner; (4) The powdered soil conditioner and the binder are mixed and granulated to obtain an easily disintegrable granular soil conditioner.
2. The method according to claim 1, characterized in that: In step (1), the silicon dioxide-rich material is selected from one or more of fly ash, coal gangue, fly ash acid-process aluminum extraction residue, and coal gasification slag.
3. The method according to claim 1 or 2, characterized in that: In step (1), the activator is selected from one or more of calcium oxide, calcium hydroxide, potassium carbonate, potassium hydroxide, sodium carbonate, magnesium oxide, brucite, and talc, preferably a combined activator comprising two or more thereof, more preferably a combined activator consisting of calcium hydroxide and sodium carbonate, and further preferably a combined activator consisting of calcium hydroxide and sodium carbonate in a mass ratio of 1:(0.18-1).
4. The method according to any one of claims 1 to 3, characterized in that: In step (1), the mass ratio of the silicon dioxide-rich material to the activator is 1:(0.7-1).
5. The method according to any one of claims 1 to 4, characterized in that: In step (1), the molding method is extrusion molding or pellet molding; and / or The volume of the granular raw material is not more than 4cm 3 .
6. The method according to any one of claims 1 to 5, characterized in that: In step (2), the activation conditions are: activation temperature 600-950° C., activation time 0.5-3 h.
7. The method according to any one of claims 1 to 6, characterized in that: In step (3), the particle size of the powdered soil conditioner is less than 200 meshes.
8. The method according to any one of claims 1 to 7, characterized in that: In step (4), the binder is selected from one or more of sodium humate, desulfurized gypsum, α-starch, and attapulgite, and the amount added is 0.5-8% of the mass of the powdered soil conditioner; and / or The particle size of the granular soil conditioner is 2-5 mm.
9. A soil conditioner prepared by the method according to any one of claims 1 to 8.
10. Use of the soil conditioner according to claim 9 in improving soil and / or as soil fertilizer.
Citation Information
Patent Citations
Disintegration-type silicon-calcium-magnesium fertilizer
CN101844949A
Multiple-effect citrate-soluble silicon fertilizer, and preparation method and application of silicon fertilizer
CN108484243A
Granular medium-trace nutrient element fertilizer and production method thereof
CN108503464A
Silicon-calcium mineral fertilizer, preparation method and application thereof
CN111217634A
Granular silicon-containing compound fertilizer and preparation method thereof
CN114057513A
Cited By
Coal gangue-based soil conditioner as well as preparation method and application thereof
CN120272203A
Silicon-based granular soil conditioner and preparation method thereof
CN120536139A