Organic-inorganic composite environment-friendly curing agent for curing shield soil and preparation method of organic-inorganic composite environment-friendly curing agent

Through the use of organic-inorganic composite environmentally friendly curing agent, the problem of low dehydration and curing efficiency of shield soil and difficulty in reducing pollutants is solved, and efficient and environmentally friendly shield soil treatment is achieved, forming high-strength and low-pollution cured soil. , meets the needs of multifunctional applications.

CN119020048AActive Publication Date: 2024-11-26SHANDONG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411136125.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

During the treatment of shield soil, there are problems such as low dehydration and curing efficiency and difficult to reduce pollutants. Traditional methods may introduce heavy metal ion pollution, and existing research cannot effectively provide solutions for shield soil pollutants.

Method used

Using organic-inorganic composite environmentally friendly curing agent, the dehydration and reinforcement of shield soil and pollutant fixation are promoted through the combination of gel-curing materials, neutral inorganic curing stabilizers, exciters and enhancers, and the solubility of heavy metal ions is reduced. Form high-strength and low-pollution solidified soil.

Benefits of technology

It realizes rapid pretreatment and centralized treatment of shield soil, reduces pollutant release rate, improves the strength and durability of cured soil, meets the needs of multifunctional applications, and reduces resource waste and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020048A_ABST
    Figure CN119020048A_ABST
Patent Text Reader

Abstract

The invention discloses an organic-inorganic composite environment-friendly curing agent for curing shield soil and a preparation method of the organic-inorganic composite environment-friendly curing agent, and relates to the technical field of shield construction. The organic-inorganic composite environment-friendly curing agent is prepared from the following raw material components in parts by mass: 2 to 2.7 parts of a gel curing material, 0.5 to 1 part of a neutral inorganic curing stabilizer, 2.3 to 2.6 parts of an exciting agent and 0.15 to 0.25 part of a reinforcing agent, wherein the neutral inorganic curing stabilizer is a water-soluble mixture containing Ca < 2 + >, K < + >, Na < + > and halide ions. The organic-inorganic composite environment-friendly curing agent disclosed by the invention can be used for reducing the retention amount of shield soil pollutants and realizing the process reduction of the pollutants, so that the shield soil is treated into recyclable soil with good engineering properties and excellent environment-friendly performance, and the green and safe utilization of the shield soil is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of shield construction, in particular to an organic-inorganic composite environmentally friendly curing agent for shield soil curing and a preparation method thereof. Background Art

[0002] With the rapid economic development and accelerated urbanization, the scale and number of urban rail transit construction are unprecedented.

[0003] The shield method is a mainstream construction method for subway tunnels. A large amount of shield spoil will be generated during the shield excavation process. The traditional method of treating shield soil is dumping, which not only occupies a large amount of precious arable land resources but also has a high treatment cost. More importantly, these shield soils contain a large amount of chemicals and clay minerals, and the total concentration of toxic chemicals can be as high as 5000mg / kg. Shield soil that has not been identified and evaluated is directly dumped into farmland or valley pits. Pollutants spread to the ecosystem with groundwater, causing chronic toxic effects on environmental organisms and human health, and seriously threatening ecological and environmental safety. From an environmental and economic perspective, there are many disadvantages in using dumping to treat shield soil. Therefore, finding a more effective and economical way to treat shield soil has become a hot issue of common concern in countries around the world.

[0004] At present, the research on shield soil performance improvement technology and materials is still in the exploratory stage. The dehydration and solidification mechanism of shield soil is still unclear. There is a single means of synergistic reduction of shield soil pollutants and low efficiency. Reactive dehydration is usually used more, and cementitious materials are generally used to treat shield soil. However, there is a risk of introducing heavy metal ion pollution when treating shield soil. There is no targeted fixation and reduction material for shield soil pollutants. The existing results mainly focus on the fixation and removal of heavy metals from site pollution. The types of shield soil and site soil pollutants are different, and the existing research results cannot provide reference for the fixation and reduction of shield soil pollutants.

[0005] Therefore, in order to achieve rapid on-site pretreatment of shield soil, centralized resource processing and green and safe utilization, it is urgent to develop environmentally friendly and efficient functional materials for improving shield soil performance and fixing and reducing pollutants. Summary of the invention

[0006] The purpose of the present invention is to provide an organic-inorganic composite environmentally friendly curing agent for shield soil curing and a preparation method thereof, so as to solve the problems that the on-site shield soil pretreatment dehydration and curing efficiency is low and it is difficult to meet the requirements for external transportation, and the shield soil pollutants are difficult to reduce and easily remain in the centralized treatment site.

[0007] To achieve the above object, the present invention provides the following solutions:

[0008] The present invention provides an organic-inorganic composite environmentally friendly curing agent for shield soil curing. The raw materials include the following components in parts by mass:

[0009] 2 to 2.7 parts of gelling and curing material, 0.5 to 1 part of neutral inorganic curing stabilizer, 2.3 to 2.6 parts of activator, and 0.15 to 0.25 parts of reinforcing agent;

[0010] The neutral inorganic curing stabilizer contains Ca 2+ , K + 、Na + and halide ions, specifically containing Ca 2+ , K + 、Na + An ion-rich, water-soluble mixture of inorganic compounds containing halide ions.

[0011] Furthermore, the gelling and solidifying material is composed of raw materials in the following mass ratio: mineral powder: quicklime: slaked lime: lime powder: dihydrate gypsum = 73-84: 2-4: 0-4: 15-25: 1.5-7.5.

[0012] In the present invention, the cementitious solidifying material is used to dehydrate and consolidate the shield soil. The composition and function of each component in the cementitious solidifying material are as follows:

[0013] Mineral powder, the main component is SiO 2 、Al 2 O 3 and CaO, and also contains a small amount of MgO, Fe 2 O 3 Other ingredients: Al 2 O 3 The higher the content of CaO and MgO, the better the activity of the mineral powder. The present invention prefers mineral powder with a total mass of more than 56%. The mineral powder has good activity, can fully participate in the curing reaction, enhance the hardening rate and strength of the gel, and reduce the heat release and alkalinity of the curing process, which plays an important role in alleviating the curing reaction and improving the performance of shield soil.

[0014] Quicklime, whose main component is CaO, has strong water absorption and can promote the dehydration and rapid setting of shield soil in the solidification process.

[0015] Slaked lime (Ca(OH) 2 ) is used as a soil acidity preventer and solidifier to reduce the acidity of shield soil, thereby improving the soil structure and performance.

[0016] Lime powder is CaCO 3It is a white powdery substance mainly composed of calcium, magnesium, iron and other elements, and other chemical substances can be added as needed to improve performance.

[0017] Gypsum dihydrate is a white powdery substance with the chemical formula of CaSO 4 ·2H 2 O. Dihydrate gypsum contains a large amount of calcium sulfate dihydrate, and also contains a small amount of impurities such as aluminum oxide, iron oxide, silicon oxide, etc. Dihydrate gypsum has good hygroscopicity, heat insulation, fire resistance and chemical corrosion resistance.

[0018] Furthermore, the activator is a mixture of water glass and sodium hydroxide in a mass ratio of 1.9-2.5:0.1-0.4; the modulus of the water glass is 1.0.

[0019] Furthermore, the enhancer is triisopropanolamine.

[0020] In the present invention, the neutral inorganic curing stabilizer promotes the hydration reaction of the cementitious curing material, reduces the water content, makes the shield soil particles more easily cemented, improves the strength and durability, produces stable hydrates (crystals), and forms a cured soil with sufficient strength. At the same time, the neutral inorganic curing stabilizer adheres to the soil particles, inhibiting the decomposition of humic acid and lignin acid in the shield soil into low molecular compounds such as alcohols and carboxylic acids.

[0021] The neutral inorganic curing stabilizer of the present invention promotes the silicon oxide (SiO 2 ) and aluminum oxide (Al 2 O 3 ) will react with the heavy metal ions in the shield soil particles to form insoluble salts, which can effectively reduce the shield soil pollutants to below the environmental benchmark value.

[0022] In the present invention, water glass can undergo polymerization reaction with shield soil, and penetrate into the shield soil to continue to undergo chemical reaction with the soil body, thereby playing a cementing role.

[0023] In the present invention, sodium hydroxide is used as an alkaline activator to activate the reaction between the cementitious solidifying material and the shield soil to generate a cementitious substance, which gradually expands and softens the surface of the soil particles, thereby making the adjacent soil particles in close contact, dissolving and bonding with each other to form a whole with higher strength, thereby improving the mechanical properties of the solidified soil.

[0024] The present invention also provides application of the organic-inorganic composite environmentally friendly curing agent in shield soil curing.

[0025] The present invention further provides a method for curing shield soil, comprising the following steps: adding the organic-inorganic composite environmentally friendly curing agent into the shield soil according to the raw material ratio, and then adding mixing water to achieve the curing of the shield soil.

[0026] Furthermore, based on the dry mass of the shield soil, the mixing ratio of the organic-inorganic composite environmentally friendly curing agent in the shield soil is 27.5% to 30%.

[0027] Furthermore, mixing water is added according to a water-solid ratio of 25% to 28%; wherein the water-solid ratio refers to the percentage of the mixing water to the dry mass of the shield soil and the total mass of the curing agent.

[0028] Furthermore, after adding mixing water, the method further comprises the step of adding a defoamer to the obtained mixture; wherein the amount of the defoamer added is preferably 3% of the mass of the obtained mixture after adding mixing water.

[0029] The defoaming agent is quicklime.

[0030] Furthermore, the mixing temperature is room temperature (18-23° C.).

[0031] In the present invention, the cementitious solidifying material, the neutral inorganic solidifying stabilizer, the activator and the reinforcing agent can react with the mixing water through a secondary hydration reaction during the shield soil solidification process to produce a stable hydrated solid, thereby improving the performance of the shield soil. Under the condition of meeting the same performance indicators, the cost is reduced by >50%; after treatment and disposal, the release rate of toxic substances in the shield soil is reduced by >50%, and the obtained solidified soil has high strength, good durability, fast solidification speed, low cost, and is environmentally friendly. It can meet the needs of different scenarios, such as backfill planting soil, sponge soil, unfired bricks, blocks, building materials, etc., and realizes the rational utilization of waste shield soil to multifunctional solidified soil.

[0032] The present invention causes shield soil to gel and solidify through hydration reaction, and simultaneously converts part of pollutant ions into insoluble crystals, so as to prepare solidified soil with high strength and little pollution.

[0033] The present invention reduces the amount of pollutant retention through multiple stages of treatment and disposal processes, thereby achieving process reduction of pollutants; and processes shield soil into reusable soil with good engineering properties and excellent environmental performance, thereby achieving green and safe utilization of shield soil.

[0034] The present invention discloses the following technical effects:

[0035] The curing agent of the present invention can process abandoned shield soil into geotechnical materials with good engineering properties, which not only solves the problem of farmland occupation caused by shield soil dumping, but also realizes resource recycling and achieves the purpose of turning waste into treasure. The prepared solidified soil product replaces building materials such as clay, sand, gravel, cement, etc., which can save costs and create indirect economic benefits.

[0036] Urban construction has a huge demand for building materials. In the past, it basically relied on conventional building materials such as clay and cement, and the production of cement is a high-energy-consuming and high-emission industry. The present invention realizes the resource utilization of shield soil, belongs to the "three wastes comprehensive utilization" industry, reduces the consumption of natural resources, promotes carbon emission reduction, and effectively realizes the differentiated utilization of building materials.

[0037] The solidified soil obtained by solidifying shield soil in the present invention has high strength, good durability, fast solidification speed, low cost and is environmentally friendly. It avoids the shortcomings of using inorganic materials such as large shrinkage, easy cracking and poor water stability, and fully utilizes the advantages of organic materials, thereby achieving effective modification of shield soil and having great market space.

[0038] The release rate of toxic substances in shield soil treated by the present invention is reduced by more than 50%, and the heavy metal ions (such as Pb 2+ 、Cd 2+ , Cu 2+ etc.) in solution with certain anions (such as OH - , CO 3 2- The heavy metals can be transformed from ionic state to crystalline state, which makes them almost incapable of being absorbed by plants and animals, and remain insoluble in groundwater for a long time. This can reduce the huge waste of resources and negative environmental effects caused by the stacking of shield soil, and realize the green and safe utilization of shield soil.

[0039] The present invention can adjust the raw material ratio to obtain curing agents with different properties, so that they show different characteristics after being cured with shield soil, so as to meet the needs of various engineering applications, such as backfill planting soil, sponge soil, unburned bricks, blocks, building materials, etc., and has a wide range of applications.

[0040] The present invention will have an all-round and far-reaching impact on building "zero-waste cities" and "low-carbon cities", promoting the improvement of urban ecological environment, reducing the emission of bulk solid waste, improving the high-value utilization of waste, reducing dependence on natural resources, helping to build a conservation-oriented society, and promoting the development of circular economy and dual-carbon strategy, and has immeasurable comprehensive benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0042] Figure 1 These are test graphs of the unconfined compressive strength of the cured soil prepared in Examples 1-6 of the present invention after 7 and 28 days of immersion and non-immersion.

[0043] Figure 2 This is a strength diagram of the solidified soil prepared in Examples 1-6 of the present invention after 5 freeze-thaw cycles.

[0044] Figure 3 This is a graph of the 28-day permeability coefficient of the solidified soil prepared in Examples 1-6 of the present invention.

[0045] Figure 4 This is a graph showing the mass loss of the solidified soils prepared in Examples 1-6 of the present invention due to sulfite corrosion.

[0046] Figure 5 This is a graph of pollutant concentration and environmental safety risk of solidified soil prepared in Examples 1-6 of the present invention. DETAILED DESCRIPTION

[0047] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0048] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0049] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0050] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0051] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0052] The "room temperature" in the present invention is 18-23°C unless otherwise specified.

[0053] The raw materials used in the following embodiments of the present invention are all commercially available products.

[0054] In the following embodiments of the present invention: Al in the mineral powder 2 O 3 , CaO and MgO account for 56% by total mass; NaOH is industrial grade, and the solid content of NaOH is ≥99%; the mixing water is drinking water; the source of shield soil (dry soil) is a shield section of Jinan Metro.

[0055] Example 1

[0056] Accurately weigh 54g of cementitious curing material, 10g of neutral inorganic curing stabilizer, 50g of water glass, 2g of sodium hydroxide, 4g of triisopropanolamine, 130g of mixing water and 400g of shield soil.

[0057] The mass ratio of each component in the cementitious solidifying material is: mineral powder: quicklime: slaked lime: lime powder: dihydrate gypsum = 77:2:3:15:3. The neutral inorganic solidifying stabilizer is CaCl 2 A mixture of KF and NaCl in a molar ratio of 7:2:1.

[0058] The solidification process of shield soil is as follows:

[0059] (1) uniformly mixing a gelling curing material, a neutral inorganic curing stabilizer and triisopropanolamine to obtain a mixture;

[0060] (2) pouring the mixture obtained in step (1) and the shield soil into a cement mortar mixer, stirring at a low speed of 60 r / min for 5 min to mix them evenly, to obtain mixed soil;

[0061] (3) Pour water glass with a modulus of 1.0 into the mixed soil of step (2), and then stir at a high speed of 120 r / min for 5 minutes; then add sodium hydroxide and mixing water to make the water-to-solid ratio reach 25%. After thorough stirring, add 3% of the mass of the obtained mixture of defoaming agent (quicklime), accelerate mixing for 2 minutes, remove bubbles in the newly mixed soil, and prepare solidified soil.

[0062] A layer of vaseline was evenly coated on the inner wall of a cylindrical mold with an inner diameter of 40 mm and a height of 80 mm. Then the solidified soil was loaded into the mold three times for compaction, and hit 20 times each time to prepare the solidified soil samples. The solidified soil samples were demolded and numbered, and placed in a curing box for curing under standard curing conditions. A total of 15 samples were prepared for 7-day and 28-day immersion and non-immersion unconfined compressive strength tests; a total of 12 samples were prepared for 28-day freeze-thaw cycle tests, permeability tests, durability tests, and pollutant dissolution tests, with 3 parallel tests in each group. A control group was also set up.

[0063] The control group used a curing agent produced by a Japanese company, the main components of which were cement: fly ash: gypsum = 4:15:3 (mass ratio). The preparation process of the cured soil was as follows:

[0064] (1) Accurately weigh 120g of curing agent, 130g of mixing water and 400g of shield soil;

[0065] (2) pouring the curing agent and shield soil obtained in step (1) into a cement mortar mixer, stirring at a low speed of 60 r / min for 5 min to mix them evenly, to obtain mixed soil;

[0066] (3) Add mixing water to the mixed soil to make the water-to-solid ratio reach 25%, accelerate the mixing at a speed of 120 r / min for 2 min, and after thorough mixing, prepare the control group solidified soil.

[0067] A layer of vaseline was evenly applied on the inner wall of a cylindrical mold with an inner diameter of 40 mm and a height of 80 mm. Then the solidified soil of the control group was loaded into the mold for compaction three times, and hit 20 times each time to prepare the control group samples of slag solidified soil. The control group samples were demoulded and numbered, and placed in a curing box for curing under standard curing conditions. A total of 15 samples were prepared for 7-day and 28-day immersion and non-immersion unconfined compressive strength tests; a total of 12 samples were prepared for 28-day freeze-thaw cycle tests, permeability tests, durability tests, and pollutant dissolution tests, with 3 parallel tests in each group.

[0068] Example 2

[0069] Accurately weigh 54g of cementitious curing material, 10g of neutral inorganic curing stabilizer, 50g of water glass, 2g of sodium hydroxide, 4g of triisopropanolamine, 130g of mixing water and 400g of shield soil.

[0070] The mass ratio of each component in the cementitious solidifying material is: mineral powder: quicklime: slaked lime: lime powder: dihydrate gypsum = 80:2:0:15:3.

[0071] The solidification process of the shield soil and the performance verification of the obtained solidified soil are the same as those in Example 1.

[0072] Example 3

[0073] Accurately weigh 44g of cementitious curing material, 15g of neutral inorganic curing stabilizer, 47g of water glass, 1g of sodium hydroxide, 3g of triisopropanolamine, 140g of mixing water and 400g of shield soil.

[0074] The mass ratio of each component in the cementitious solidifying material is: mineral powder: quicklime: slaked lime: lime powder: dihydrate gypsum = 77:2:3:15:3.

[0075] The solidification process of the shield soil and the performance verification of the obtained solidified soil are the same as those in Example 1.

[0076] Example 4

[0077] Accurately weigh 48g of cementitious curing material, 15g of neutral inorganic curing stabilizer, 48g of water glass, 3g of sodium hydroxide, 5g of triisopropanolamine, 131g of mixing water and 400g of shield soil.

[0078] The mass ratio of each component in the cementitious solidifying material is: mineral powder: quicklime: slaked lime: lime powder: dihydrate gypsum = 77:2:3:15:3.

[0079] The solidification process of the shield soil and the performance verification of the obtained solidified soil are the same as those in Example 1.

[0080] Example 5

[0081] Accurately weigh 46g of cementitious curing material, 18g of neutral inorganic curing stabilizer, 45g of water glass, 1g of sodium hydroxide, 4g of triisopropanolamine, 136g of mixing water and 400g of shield soil.

[0082] The mass ratio of each component in the cementitious solidifying material is: mineral powder: quicklime: slaked lime: lime powder: dihydrate gypsum = 77:2:3:15:3.

[0083] The solidification process of the shield soil and the performance verification of the obtained solidified soil are the same as those in Example 1.

[0084] Example 6

[0085] Accurately weigh 46g of cementitious curing material, 20g of neutral inorganic curing stabilizer, 46g of water glass, 4g of sodium hydroxide, 3g of triisopropanolamine, 131g of mixing water and 400g of shield soil.

[0086] The mass ratio of each component in the cementitious solidifying material is: mineral powder: quicklime: slaked lime: lime powder: dihydrate gypsum = 77:2:3:15:3.

[0087] The solidification process of the shield soil and the performance verification of the obtained solidified soil are the same as those in Example 1.

[0088] Figure 1 The unconfined compressive strength test diagrams of the solidified soil prepared in Example 1-6 (Case 1-6) of the present invention for 7 days and 28 days of immersion and non-immersion. The results show that the compressive strength of the solidified soil obtained by consolidating the shield soil using the solidifying agent of the present invention is greatly improved. The reason why the solidifying agent of the present invention can improve the strength of the solidified soil is that the solid particles in the solidified soil are composed of inorganic mineral particles, mainly including limestone, silica and calcium feldspar, etc., which have stable physical and chemical properties and low internal activity; the amount of mineral powder in the solidifying agent is relatively large, so that the mixed soil has a higher hydration activity. During the solidification process, limestone and silica participate in the reaction to generate hydrated calcium silicate and hydrated calcium sulfoaluminate. The hydrated calcium sulfoaluminate crystals overlap each other, and the hydrated calcium silicate gel cross-climbs, connecting the dispersed shield soil particles together to form a dense three-dimensional spatial structure, which increases the compressive strength of the solidified soil. At the same time, water glass acts as an activator, which makes the active SiO 2 The increase of OH- content accelerates the excitation and reaction speed, which is beneficial to the polymerization reaction of the material; triisopropanolamine as a reinforcing agent promotes the Ca 2+ 、Al 3+ 、Si 4+ The rate of ion dissolution will also be conducive to the formation of gels such as hydrated calcium silicate, thereby improving the compressive strength.

[0089] Figure 2 The strength diagram of the solidified soil prepared in Example 1-6 (Case 1-6) of the present invention after 5 freeze-thaw cycles. The results show that the strength loss rate of the solidified soil in Example 1-6 of the present invention is much lower than that of the conventional solidified soil, and the antifreeze effect is significant.

[0090] Figure 3 The permeability coefficient of the solidified soil prepared in Example 1-6 (Case 1-6) of the present invention after 28 days is shown in Figure 1. The results show that the permeability coefficient of the solidified soil prepared in the present invention is significantly lower than that of the conventional solidified soil, and the anti-seepage effect is greatly improved.

[0091] The preparation of highly permeable building materials can be achieved by increasing the amount of quicklime, reducing the amount of water glass, shortening the mixing time, etc.

[0092] Figure 4 The graph of mass loss of the stabilized soil prepared in Example 1-6 (Case 1-6) of the present invention due to sulfurous acid erosion shows that the durability of the stabilized soil prepared in Example 1-6 of the present invention is up to nearly 7 times that of the conventional stabilized soil.

[0093] Figure 5 The pollutant concentration and environmental safety risk diagram of the solidified soil prepared in Example 1-6 (Case 1-6) of the present invention. The results show that the pollutant concentration and environmental safety risk of the solidified soil prepared by the present invention are significantly lower than those of the untreated shield soil.

[0094] In terms of compressive strength, the performance of Example 1 of the present invention is the best, and the prepared solidified soil has high strength, with unconfined compressive strengths of 4.98 MPa and 9.54 MPa at 7 days and 28 days, respectively, while the unconfined compressive strengths of the control group at 7 days and 28 days are 1.55 MPa and 2.24 MPa, respectively; the solidified soil of Example 1 of the present invention has the best durability, with a mass loss rate of only 1%, which is about 6 times higher than that of the control group at 6.7%.

[0095] The curing agent in Example 1 corresponds to the following dosage of each raw material in the shield soil: the dosage of cementitious curing material is 8.3% (mineral powder: quicklime: slaked lime: lime powder: dihydrate gypsum = 77:2:3:15:3), the dosage of neutral inorganic curing stabilizer is 1.5%, the water glass modulus is 1.0, the dosage of water glass is 8.0%, the dosage of triisopropanolamine is 0.6%, and the dosage of mixing water is 20%.

[0096] According to the requirements for the unconfined compressive strength of cured soil at 7d age in the "Technical Code for Application of Road Cured Soil" T / CECS737-2020, the cured soils of Examples 1-6 can all be used as road subgrade filling materials.

[0097] According to the Technical Specification for Channel Anti-seepage Engineering SL / 18-2004, the permeability coefficients of the solidified soils in Examples 1-6 are all less than 1×10 -6 cm / s, and can be used as channel anti-seepage material for seasonal and year-round water delivery in areas with mild climate and no frost damage.

[0098] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. An organic-inorganic composite environmentally friendly curing agent for shield soil curing, characterized in that: The raw materials include the following components in terms of mass: 2 to 2.7 parts of gelling and curing material, 0.5 to 1 part of neutral inorganic curing stabilizer, 2.3 to 2.6 parts of activator, and 0.15 to 0.25 parts of reinforcing agent; The neutral inorganic curing stabilizer contains Ca 2+ , K + 、Na + A water-soluble mixture of ions and halide ions.

2. The organic-inorganic composite environmentally friendly curing agent according to claim 1, characterized in that: The gelling and solidifying material is composed of raw materials in the following mass ratio: mineral powder: quicklime: slaked lime: lime powder: dihydrate gypsum = 73-84: 2-4: 0-4: 15-25: 1.5-7.

5.

3. The organic-inorganic composite environmentally friendly curing agent according to claim 1, characterized in that: The activator is a mixture of water glass and sodium hydroxide in a mass ratio of 1.9-2.5:0.1-0.4; the modulus of the water glass is 1.0-1.

3.

4. The organic-inorganic composite environmentally friendly curing agent according to claim 1, characterized in that: The enhancer is triisopropanolamine.

5. Use of the organic-inorganic composite environmentally friendly curing agent as described in any one of claims 1 to 4 in shield soil curing.

6. A method for solidifying shield soil, characterized in that: The method comprises the following steps: adding the organic-inorganic composite environmentally friendly curing agent described in any one of claims 1 to 4 into shield soil according to the raw material ratio, and then adding mixing water to realize the curing of the shield soil.

7. The curing method according to claim 6, characterized in that: Calculated on the dry mass of the shield soil, the mixing ratio of the organic-inorganic composite environmentally friendly curing agent in the shield soil is 27.5% to 30%.

8. The curing method according to claim 6, characterized in that: Add mixing water according to the water-to-solid ratio of 25% to 28%.

Citation Information

Patent Citations

  • Soft soil curing agent

    CN101215141A

  • High-humic-acid multi-solid-waste coupling soft soil curing agent in cold region

    CN114031362A

  • Aerated concrete and preparation method thereof

    CN115849940A

  • Soil stabilizer as well as preparation method and application thereof

    CN116573900A