Composition and method for removing residues after ashing of semiconductor substrate

The safety in the prior art is solved by removing the ash residue of the semiconductor substrate at low temperature by free of fluoride and hydroxylamine, which combines a wetting agent and phenolic corrosion inhibitor. Hidden dangers and corrosion problems have achieved efficient and low-cost cleaning results.

CN119020117AActive Publication Date: 2024-11-26XIN SHI DA DIAN ZI CAI LIAO (KUN SHAN) YOU XIAN GONG SI
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411120991.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Existing semiconductor cleaning agents have safety hazards when removing the residue after ash, they cannot effectively control the corrosion of the substrate material, have poor removal effect on inorganic metal residues, and have high operating temperatures or safety risks, which affects the electrical performance and reliability of semiconductors. sex.

Method used

A composition is provided, including 0.05-10 wt% organic amine compound, 0.001-10 wt% wetting agent and 80-99.5 wt% water, for removing residues after dry etching plaster ash at low temperature. The composition, free of fluoride and hydroxylamine, contains phenolic corrosion inhibitors to reduce metal corrosion rates and control pH between 10-12.

Benefits of technology

Effectively remove the ashed residue of semiconductor substrates under low temperature conditions, reduces the metal erosion rate, improves the cleaning efficiency, avoids safety hazards and substrate corrosion, and is suitable for the new generation of single-chip cleaning machines, reducing production costs and Energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020117A_ABST
    Figure CN119020117A_ABST
Patent Text Reader

Abstract

The invention discloses a composition and a method for removing residues after ashing of a semiconductor substrate, the composition comprises 0.05-10 wt% of an organic amine compound, 0.001-10 wt% of a wetting agent and 80-99.5 wt% of water, and the wetting agent comprises at least one of a polyol compound or a surfactant. The water-based cleaning agent is free of hydroxylamine and fluoride, takes an organic amine compound as a main body, is matched with a wetting agent (a polyhydric alcohol compound and / or a surfactant) and water to form the water-based cleaning agent, does not contain a large amount of organic solvent, does not contain a chelating agent or a silicate corrosion inhibitor, and is lower in cost and environment-friendly. The cleaning agent has the advantages of low temperature operation, difficult loss of moisture and effective components in the cleaning agent, good composition stability, low metal erosion rate and stable cleaning efficiency, can effectively remove residues after dry etching plasma ashing, and does not erode or slightly erode metal lines, dielectric layers and wafer substrate materials on original wafers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor cleaning, and in particular relates to a composition and a method for removing residues after ashing of a semiconductor substrate. Background Art

[0002] In the manufacture of semiconductor integrated circuits, photolithography technology (coating, exposure, development and etching of photoresist layers) is required to form fine electronic circuit patterns on substrates. During the patterning process, residues will remain on the surface of the semiconductor substrate. Before the next step after the patterning process, the etching residues need to be removed or cleaned. This removal or cleaning is usually referred to as "post-etching residue" removal or "post-ashing residue" removal in the industry. These residues can cause short circuits between wirings or cause poor connection during the deposition of metal or dielectric layers in subsequent processes, which adversely affects the electrical properties of semiconductors. Therefore, these residues need to be thoroughly removed or cleaned. If they are not removed or cleaned thoroughly, the electrical performance and reliability of semiconductor devices may be reduced.

[0003] The industry usually uses wet cleaning to remove or clean the residue after ashing. Existing traditional cleaning agents mainly include hydroxylamine, fluorine, semi-aqueous amine (without hydroxylamine) and water-based cleaning agents.

[0004] Hydroxylamine cleaning fluids have good cleaning effects and are widely used in semiconductor cleaning and other fields because hydroxylamine and its salts are important chemical raw materials. However, hydroxylamine has low stability and is prone to explosion at high operating temperatures. This makes hydroxylamine cleaning fluids pose a greater safety hazard during preparation and use.

[0005] Fluorine cleaning agents generally include fluoride + amine compounds + organic solvents + water. Fluorine cleaning agents can be cleaned at lower temperatures (room temperature to 50°C), but there are still some disadvantages, such as the inability to control the corrosion of the base material well. Fluorides such as ammonium fluoride or hydrofluoric acid are extremely harmful to the human body in an acidic environment. Direct contact is toxic. If not immediately treated, it will cause bone erosion. Long-term inhalation will cause osteoporosis in the human body, posing a great safety risk.

[0006] Semi-aqueous amine cleaners are mainly organic amines and organic stripping solvents, water and metal corrosion inhibitors. However, these cleaners usually have a high operating temperature (50-90°C), and they are less effective in removing inorganic metal residues, so they are not widely used.

[0007] The water-based cleaning solution mainly includes metal ion-free alkali, silicate corrosion inhibitor, metal oxoate, chelating agent and water, operates at low temperature and is environmentally friendly. However, existing water-based cleaning agents also have some defects. For example, silicate corrosion inhibitors increase the viscosity of the cleaning solution and are not conducive to the cleaning of fine line widths or tiny holes on chip structures. During the cleaning process, the chemical bonding generated by silicate corrosion inhibitors may cause discoloration and contamination of some substrates. At the same time, as the pH value decreases, it will hydrolyze to produce particles and contaminate the wafer. This is why the present invention comes from this. Summary of the invention

[0008] In view of at least one of the above-mentioned technical problems, the object of the present invention is to provide a composition and method for removing residues after ashing of a semiconductor substrate, wherein the composition does not contain fluoride or hydroxylamine, and can effectively remove residues after dry etching plasma ashing when operated at a relatively low temperature (below 50°C), without corroding or causing extremely low corrosion to the metal circuits, dielectric layers and wafer substrate materials originally on the wafer.

[0009] The technical solution of the present invention is:

[0010] One of the objects of the present invention is to provide a composition for removing residues after ashing of a semiconductor substrate, which comprises, by weight percentage, 0.05-10wt% of an organic amine compound, 0.001-10wt% of a wetting agent and 80-99.5wt% of water, wherein the wetting agent comprises at least one of a polyol compound or a surfactant.

[0011] Preferably, the organic amine compound includes at least one of N-methylethanolamine, monoethanolamine, diethanolamine, triethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, 2-(2-aminoethoxy)ethanol, N-ethylethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, N-methyldiethanolamine, N-ethyldiethanolamine, cyclohexylaminediethanol, and quaternary ammonium hydroxide.

[0012] Preferably, the quaternary ammonium hydroxide includes at least one of tetramethylammonium hydroxide and tetraethylammonium hydroxide.

[0013] Preferably, the polyol compound includes at least one of ethylene glycol, propylene glycol, glycerol, polyethylene glycol and polypropylene glycol.

[0014] Preferably, 0.1-10 wt % of a phenolic corrosion inhibitor is also included.

[0015] Preferably, the phenolic corrosion inhibitor includes at least one of tert-butylcatechol, catechol, resorcinol, 2,3-dihydroxybenzoic acid, and gallic acid.

[0016] Preferably, it has a pH value of 10-12.

[0017] Preferably, its operating temperature is 10 to 50°C.

[0018] One of the objects of the present invention is to provide a method for removing residues after ashing of a semiconductor substrate, wherein the surface of the semiconductor substrate from which the residues after ashing are to be removed is contacted with any of the above-mentioned compositions.

[0019] Preferably, the temperature of the composition when in contact with the surface of the semiconductor substrate is 10-50°C.

[0020] Compared with the prior art, the advantages of the present invention are:

[0021] The composition and method for removing residues after ashing of semiconductor substrates of the present invention do not contain hydroxylamine, which can solve the potential safety hazard caused by the explosion of hydroxylamine; do not contain fluoride, which can solve the safety risk of fluoride. The water-based cleaning agent is mainly composed of organic amine compounds, a wetting agent (polyol compound and / or surfactant) and water, which does not contain a large amount of organic solvents, nor does it contain chelating agents and silicate corrosion inhibitors, and is lower in cost and environmentally friendly. The composition is operated at a low temperature (10 to 50° C.), and the water and effective ingredients in the cleaning agent are not easy to dissipate. The composition has good stability, a low metal corrosion rate, stable cleaning performance, and can effectively remove residues after dry etching plasma ashing, and has no or very low corrosion to the metal circuits, dielectric layers and wafer substrate materials on the original wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:

[0023] Figure 1 It is a schematic diagram of the corrosion rate of aluminum at different temperatures of the composition for removing residues after ashing of a semiconductor substrate according to Example 1 of the present invention;

[0024] Figure 2 This is an electron microscope photograph of a SRO / TEOS / SiN semiconductor structure before cleaning using the composition for removing residues after ashing of a semiconductor substrate according to Example 11 of the present invention;

[0025] Figure 3 This is an electron microscope photograph of a SRO / TEOS / SiN semiconductor structure after cleaning with the composition for removing residues after ashing of a semiconductor substrate according to Example 11 of the present invention;

[0026] Figure 4 This is an electron microscope photograph of a TiW / Al semiconductor structure before cleaning using the composition for removing residues after ashing of a semiconductor substrate according to Example 11 of the present invention;

[0027] Figure 5This is an electron microscope photograph of a TiW / Al semiconductor structure after cleaning with the composition for removing residues after ashing of a semiconductor substrate according to Example 11 of the present invention. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0029] The composition for removing the residue after the semiconductor substrate is ashed according to the embodiment of the present invention comprises 0.05-10wt% of an organic amine compound, 0.001-10wt% of a wetting agent and 80-99.5wt% of water according to weight percentage, wherein the wetting agent comprises at least one of a polyol compound or a surfactant, and does not contain hydroxylamine, fluoride, a large amount of organic solvent, organic carboxylic acid chelating agent and silicate corrosion inhibitor. The above-mentioned component reagents are all chemical reagents that can be purchased on the market or are well known to those skilled in the art.

[0030] According to some preferred embodiments of the present invention, the organic amine compound preferably includes at least one of N-methylethanolamine, monoethanolamine, diethanolamine, triethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, 2-(2-aminoethoxy)ethanol, N-ethylethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, N-methyldiethanolamine, N-ethyldiethanolamine, cyclohexylaminediethanol, and quaternary ammonium hydroxide. The specific organic amine compounds mentioned above are all chemical reagents that can be purchased on the market or are well known to those skilled in the art. Further preferably, the quaternary ammonium hydroxide includes at least one of tetramethylammonium hydroxide and tetraethylammonium hydroxide.

[0031] According to some preferred embodiments of the present invention, the polyol compound includes at least one of ethylene glycol, propylene glycol, glycerol, polyethylene glycol, and polypropylene glycol. The above-mentioned specific polyol compounds are all chemical reagents that can be purchased on the market or are well known to those skilled in the art. Surfactants are compounds that contain both hydrophilic groups and lipophilic groups in molecules such as common soaps and shampoos on the market. For example, in some embodiments of the present invention, the surfactant Triton X-100 (polyethylene glycol octylphenyl ether) is used. When the wetting agent is a compound of a polyol compound and a surfactant, the specific ratio of the two is not particularly limited and can be selected as 1:1.

[0032] According to some preferred embodiments of the present invention, the composition can also be compounded with a phenolic corrosion inhibitor, rather than the silicate corrosion inhibitor of the prior art. The addition of phenolic corrosion inhibitors can further improve the protection of aluminum and copper materials, that is, further reduce the corrosion of aluminum and copper materials. Preferably, the content of phenolic corrosion inhibitors in the formula is 0.1-10wt% by weight. The embodiment of the present invention optimizes and controls the content of phenolic corrosion inhibitors, and does not have a significant impact on the pH value of the formula while improving the protection. Exemplarily, the phenolic corrosion inhibitors of the embodiments of the present invention are selected from at least one of tert-butylcatechol, catechol, resorcinol, 2,3-dihydroxybenzoic acid, and gallic acid. The specific phenolic corrosion inhibitors mentioned above are all chemical reagents that can be purchased on the market or are well known to those skilled in the art.

[0033] According to some preferred embodiments of the present invention, the composition has a pH value of 10-12. Since the composition is mainly composed of organic amine compounds, it is alkaline. By optimizing the formula and controlling the amount of wetting agent and water, the pH value of the formula is 10-12. Compared with existing acidic cleaning agents, the corrosion of aluminum, copper and other wires is smaller. Moreover, by controlling the pH value, the composition can have no corrosion or very low corrosion on the metal circuits, dielectric layers and wafer substrate materials on the original wafer.

[0034] According to some preferred embodiments of the present invention, the operating temperature of the composition is 10 to 50°C. Since the composition of the present invention is a water-based cleaning agent, the proportion of water is very large, and low-temperature operation can reduce the loss of water and effective components in the cleaning agent, thereby making the composition more stable and having extremely high cleaning energy efficiency. Compared with existing cleaning agents such as DuPont EKC-270, which require an operating temperature of 60-80°C, the operating temperature of the composition of the present invention is milder and the energy consumption is lower.

[0035] The applicant has found through research that the composition of the embodiment of the present invention has a fast reaction speed and high removal efficiency (30-300 seconds) when used to remove residues after ashing of semiconductor substrates. It is not suitable for operation on traditional slot machines because there will be a time difference in pulling all chip racks away, which will lead to differences between chips. However, it is very suitable for single-chip cleaning machines in the new generation of processes because single-chip cleaning machines can accurately control the process time, which enables the composition of the embodiment of the present invention to play the greatest benefit, thereby greatly improving production efficiency and reducing production cycle and production cost.

[0036] The advantages and rationality of the composition of the present invention are explained below in conjunction with specific examples, as shown in Tables 1 to 4.

[0037] Table 1 Formulations of the compositions of Examples 1 to 20 and the aluminum corrosion rates at an operating temperature of 25°C

[0038]

[0039]

[0040] Note: “-” in the table means not contained or not added. The average molecular weight of polyethylene glycol-200 is 200 g / mol.

[0041] Table 1 is an embodiment of the composition formula of the embodiment of the present invention. It can be seen from the aluminum erosion rate test results of Examples 1 to 7 in Table 1 that when the composition containing only monoethanolamine is used for cleaning semiconductor substrates, the aluminum erosion rate is significantly lower than that of the composition containing only tetramethylammonium hydroxide (Examples 1 and 5). When a mixture of monoethanolamine and tetramethylammonium hydroxide is used as the composition of the organic amine compound (Examples 2 to 4 and Examples 6 and 7), when the amount of monoethanolamine is higher than that of tetramethylammonium hydroxide, the aluminum erosion rate is significantly lower and as the ratio of monoethanolamine to tetramethylammonium hydroxide increases, the erosion rate decreases, and after reaching a certain ratio (the ratio of the two in Example 7 of the present invention is 5:1, which is lower than that in Example 1, and the ratio of the two in Example 6 is 2:1, which is higher than that in Example 1), it is lower than that of the composition containing only monoethanolamine. Therefore, the applicant has obtained through optimization that the amount of organic amine compound used is 0.05-10wt%, which can ensure extremely high cleaning energy efficiency and low cost.

[0042] Examples 8 to 13 are compared with Example 6, specifically, they are examples in which different types of polyol compounds are added to Example 6 (Examples 8 to 11 all add a polyol compound, Example 12 adds a surfactant, and Example 13 adds both a polyol compound and a surfactant). From the aluminum erosion rate test results, it can be seen that the aluminum erosion rate of the composition with the addition of the polyol compound is lower than that of the examples without the addition of the polyol compound (i.e., Examples 1 to 7), and the aluminum erosion rate of the composition after the polyol compound and the surfactant are added at the same time is greatly reduced compared with the addition of the polyol compound alone, indicating that the addition of the wetting agent can reduce the aluminum erosion rate and the compounding of the polyol compound and the surfactant can further reduce the aluminum erosion rate.

[0043] From Examples 14 to 16, it can be seen that as the amount of polyol compound increases, the aluminum corrosion rate will gradually decrease, but the reduction is relatively small. Therefore, the applicant has optimized the amount of wetting agent to ensure extremely high cleaning efficiency at 0.001-10wt%, and can also reduce the cost.

[0044] It can be seen from Examples 17 to 20 that Examples 17 to 20 are compositions in which different phenolic corrosion inhibitors are added to Example 11. It can be seen from the aluminum corrosion rate test results that the addition of phenolic corrosion inhibitors can further slow down the aluminum corrosion rate without affecting the cleaning effect. Therefore, the applicant has obtained the best amount of phenolic corrosion inhibitors by optimization, which can ensure extremely high cleaning efficiency and low cost at 0.1-10wt%.

[0045] Table 2 Cleaning time of the compositions of Examples 1 to 20 for removing residues of various materials after plasma ashing (temperature 25° C., unit: seconds)

[0046] aluminum Silicon Nitride Titanium Nitride Example 1 30 120 180 Example 2 15 60 90 Example 3 <15 60 90 Example 4 <15 30 60 Example 5 <15 30 60 Example 6 15 90 120 Example 7 30 120 180 Example 8 45 180 240 Example 9 30 120 180 Example 10 60 240 300 Embodiment 11 45 180 240 Example 12 180 360 >600 Embodiment 13 180 300 >600 Embodiment 14 45 180 240 Embodiment 15 60 210 300 Example 16 90 240 360 Embodiment 17 60 180 240 Embodiment 18 90 240 300 Embodiment 19 60 180 240 Embodiment 20 90 240 300

[0047] As can be seen from Table 2, the composition of the embodiment of the present invention is used to remove the residues after plasma ashing of semiconductors of various materials in a cleaning time of less than 600 seconds, especially for aluminum material, the time is even shorter, less than 60 seconds, which means the reaction speed is fast.

[0048] Table 3 Corrosion rate of the compositions of Examples 8 to 13 on different metals (Unit 25℃)

[0049]

[0050] In order to verify the reliability of the composition of the embodiment of the present invention, as shown in Table 3, the applicant also verified the erosion rate of the composition of Examples 8 to 13 on different metals. As shown in Table 3, the composition of Examples 8 to 13 has very little erosion on metals such as aluminum, copper, silicon oxide film made of electronic grade tetraethyl orthosilicate (TEOS), low-K insulating material, silicon nitride, titanium nitride and silicon oxide film (Thermal oxide) made at high temperature. This verifies that the composition of the present invention can be used for cleaning and removing residues after ashing of semiconductor substrates.

[0051] Furthermore, in order to further verify the optimal operating temperature of the composition of the embodiment of the present invention for removing the residue after plasma ashing of the semiconductor substrate, the applicant selected Example 11 as the formula of the optimized composition and used it to remove the residue after ashing of the semiconductor substrate. In order to verify the optimal process parameters of the composition of Example 11 for removing the residue after ashing of the semiconductor substrate, the applicant conducted the following experiment: Figure 1 The corrosion rate of aluminum using the composition of Example 5 at different temperatures is verified. Figure 1 It can be seen that the applicant found that the aluminum corrosion rate of the composition of Example 11 was relatively small (less than ), however, when the temperature exceeds 50°C, such as 60°C, the aluminum corrosion rate increases significantly, and at 10°C below room temperature, the aluminum corrosion rate also has excellent performance. Therefore, the applicant verified that the operating temperature of the composition of the embodiment of the present invention for removing residues is 10°C to 50°C. If the operating temperature is too low and residues remain during the removal process, it is recommended that the operating temperature be controlled at no more than 50°C.

[0052] Conventional organic amine compound cleaning agents generally contain multifunctional organic acids (such as phthalic acid, oxalic acid, ethylenediaminetetraacetic acid-disodium (EDTA-2Na)) as chelating agents, which are used to chelate the metals in the aqueous solution of the composition, so as to chelate the metal ions precipitated / dissolved on the chip after the semiconductor is cleaned. In theory, after adding multifunctional organic acids to the formula of the composition of the embodiment of the present invention, the stability and cleaning efficiency of the composition will all increase. However, the applicant found that, as shown in Table 4 below, after adding a certain amount of multifunctional organic acids to the formula of the composition of the present invention, the aluminum corrosion rate not only did not decrease, but increased. Therefore, the formula of the present application does not contain multifunctional organic acids, which not only reduces the cost, but also has better cleaning efficiency. That is to say, the composition of Example 11 of the present invention has a lower aluminum corrosion rate and better protection for the aluminum circuits on the cleaned chip.

[0053] Table 4 Formula table of the composition of Example 11 of the present invention and Comparative Examples 1 to 3

[0054]

[0055] Note: “-” in the table means not contained or not added. The average molecular weight of polyethylene glycol-200 is 200 g / mol.

[0056] After a high load wafer cleaning volume of 25 12-inch wafers per liter, the composition of Example 11 of the present invention can also achieve the removal effect of the plasma ashing residue on the wafer and a lower aluminum erosion rate. At the same time, the aluminum etching rate can also be controlled within This result shows that without the addition of multifunctional organic acid, the composition of Example 11 still has excellent solution stability, and the cleaning of the wafer can still achieve the desired effect, while also having a lower aluminum corrosion rate. In summary, the composition of the embodiment of the present invention has better protection for the aluminum circuit on the cleaned wafer.

[0057] The present invention also provides a method for removing residues from a semiconductor substrate after ashing, wherein the surface of the semiconductor substrate from which the residues are to be removed is contacted with the composition of the above embodiments 1 to 20. In order to achieve a better removal effect, the temperature of the composition when in contact with the surface of the semiconductor substrate is 10 to 50°C.

[0058] Figures 2 to 5 Different semiconductor structures are also given (including Figure 2 and Figure 3 It is a SRO / TEOS / SiN semiconductor structure. Figure 4 and Figure 5 The TiW / Al semiconductor structure was cleaned with the composition of Example 11 at 25°C to remove the residue after ashing ( Figure 2 and Figure 4 Before removing, Figure 3 for Figure 5 After removal, Figure 3 The cleaning time is 180 seconds. Figure 5 Electron microscope photo of the cleaning time of 45 seconds. Figure 2 and Figure 3 It is known that Figure 2 The wafer before processing is shown to be full of dot-shaped residues from dry etching plasma ashing. Figure 3 The residue on the display wafer has been removed. Figure 4 The display chip is covered with the residues after the dry etching plasma ashing. Figure 5 The residue on the display wafer has been removed.

[0059] The sources and specifications of the raw materials in Examples 1 to 20 and Comparative Examples 1 to 3 of the present invention are as follows in Table 5:

[0060] Table 5 Raw material sources and specifications

[0061]

[0062] The specified directions in this specific embodiment are only for the convenience of describing the positional relationship and the coordination relationship between the components. The above is only a preferred embodiment of the present invention. The protection scope of the present invention is not limited to the above embodiment. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A composition for removing residues after ashing of a semiconductor substrate, characterized in that: The invention comprises 0.05-10 wt % of an organic amine compound, 0.001-10 wt % of a wetting agent and 80-99.5 wt % of water according to weight percentage, wherein the wetting agent comprises at least one of a polyol compound or a surfactant.

2. The composition according to claim 1, characterized in that The organic amine compound includes at least one of N-methylethanolamine, monoethanolamine, diethanolamine, triethanolamine, monoisopropanolamine, diisopropanolamine, triisopropanolamine, 2-(2-aminoethoxy)ethanol, N-ethylethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, N-methyldiethanolamine, N-ethyldiethanolamine, cyclohexylaminediethanol, and quaternary ammonium hydroxide.

3. The composition according to claim 2, characterized in that The quaternary ammonium hydroxide includes at least one of tetramethylammonium hydroxide and tetraethylammonium hydroxide.

4. The composition according to claim 1, characterized in that The polyol compound includes at least one of ethylene glycol, propylene glycol, glycerol, polyethylene glycol, and polypropylene glycol.

5. The composition according to any one of claims 1 to 4, characterized in that Also included is 0.1-10 wt % of a phenolic corrosion inhibitor.

6. The composition according to claim 5, characterized in that The phenolic corrosion inhibitor includes at least one of tertiary butylcatechol, catechol, resorcinol, 2,3-dihydroxybenzoic acid and gallic acid.

7. The composition according to claim 1, characterized in that It has a pH value of 10-12.

8. The composition according to claim 1, characterized in that Its operating temperature is 10 to 50°C.

9. A method for removing residues after ashing of a semiconductor substrate, characterized in that: The surface of the semiconductor substrate from which the residue after ashing is to be removed is contacted with the composition according to any one of claims 1 to 8.

10. The method according to claim 9, characterized in that The temperature of the composition when in contact with the surface of the semiconductor substrate is 10-50°C.

Citation Information

Patent Citations

  • Water-rich cleaning solution composition for photoresist residue

    CN106933067A

  • Water-based micro-electronic stripping and cleanout fluid composition

    CN107338126A

  • Water-based stripping liquid composition and use method thereof

    CN113741158A

  • Semi-water-based wafer substrate cleaning solution composition and use method thereof

    CN115895800A

  • Composition and method for removing residues and photoresist after ashing of semiconductor substrate

    CN117590709A